Chemical Analysis
Typical Values (Weight %)
| Nickel | 34.0 - 37.0 | Chromium | 17.0 - 20.0 |
| Iron | Balance* | Carbon | 0.08 max. |
| Silicon | 0.75 - 1.50 | Manganese | 2.0 max. |
| Phosphorus | 0.030 max. | Sulfur | 0.030 max. |
Thermal and Electrical Properties
| Temperature | Thermal Conductivity | Electrical Resistivity | |||
| °F | °C | Btu-in/ft2M/-h-°F | W/m-°C | ohm-circ mil/ft | mW-m |
| 75 | 24 | 86 | 12.4 | 612 | 1.017 |
| 400 | 204 | 108 | 15.6 | 649 | 1.079 |
| 800 | 227 | 134 | 19.3 | 688 | 1.144 |
| 1200 | 649 | 162 | 23.4 | 721 | 1.199 |
| 1600 | 871 | 198 | 28.6 | 744 | 1.237 |
| 1800 | 982 | 216 | 31.2 | 749 | 1.245 |
Mechanical Properties
Typical Room Temperature Mechanical Properties, Mill Annealed
| Yield Strength 0.2% Offset |
Ultimate Tensile Strength |
Elongation in 2 inches (50mm) |
Hardness | ||
| ksi | (MPa) | ksi | (MPa) | % | Rockwell B |
| 30 - 43 | 207 - 296 | 80 - 85 | 552 - 586 | 40 - 45 | 70 – 85 |