Q355 and ASTM A572 at a Glance
Q355 is a low-alloy high-strength structural steel specified in GB/T 1591, with a guaranteed yield strength of 355 MPa in sections up to 16 mm. It is produced as hot-rolled plate, coil and strip, and is one of the most common structural grades for steel buildings, bridges, ship hulls, pressure equipment supports and general machinery in projects designed to Chinese standards. ASTM A572 Grade 50 is the closest US counterpart: it guarantees a minimum yield strength of 345 MPa (50 ksi) and is widely used for bolted and welded structures in North American and Middle East projects. The two grades sit at the same strength level, but their chemical limits, tolerances and testing requirements differ, so substitution always needs design verification.
Chemical Composition and What It Means
The table below lists the main element limits for Q355B per GB/T 1591 and for Grade 50 per ASTM A572/A572M. Carbon and sulphur limits are the most important controls for weldability, while manganese provides strength and offsets the harmful effect of sulphur by forming manganese sulphide inclusions.
| Element (max %) | Q355B (GB/T 1591) | A572 Gr.50 (ASTM A572/A572M) |
|---|---|---|
| C | 0.20 | 0.23 |
| Si | 0.50 | 0.15-0.40 |
| Mn | 1.60 | 1.35 |
| P | 0.035 | 0.04 |
| S | 0.035 | 0.05 |
Within the Q355 family, the letter after Q355 marks the quality grade and the required impact test temperature: Grade A and B set no low-temperature impact requirement, Grade C requires 34 J at 0 degrees C, Grade D at -20 degrees C, and Grade E at -40 degrees C. Phosphorus and sulphur limits tighten from Grade A (P and S max 0.045%) to Grade E (P max 0.025%, S max 0.020%), which improves weldability and low-temperature toughness for winter construction and offshore service.
Mechanical Properties by Thickness
Yield strength in both standards decreases as thickness increases, because thicker plates receive less total rolling reduction and cool differently. The following values for Q355 are taken from the GB/T 1591 property table; tensile strength stays at 470-630 MPa across the common range and elongation A is thickness-dependent (about 20-21% in lighter sections).
| Thickness t (mm) | Yield strength ReH (MPa, min) | Tensile Rm (MPa) |
|---|---|---|
| t ≤ 16 | 355 | 470-630 |
| 16 < t ≤ 40 | 345 | 470-630 |
| 40 < t ≤ 63 | 335 | 470-630 |
| 63 < t ≤ 80 | 325 | 470-630 |
For comparison, Q235 (GB/T 700) guarantees only 235 MPa yield and is a plain carbon structural grade, while ASTM A36 guarantees 250 MPa (36 ksi). Selecting Q355 or A572 Gr.50 instead of Q235 or A36 typically allows a lighter section for the same design load, which reduces dead weight and long-term steel cost even though the unit price per tonne is higher.
Delivery Conditions and Forms
Q355 plate and coil can be supplied in several delivery conditions: hot-rolled (as-rolled), controlled-rolled, normalized or thermomechanically processed. Hot-rolled coil (HRC) is the most economical form for slitting, blanking and cold forming; controlled rolling and normalizing refine the grain structure and improve toughness for thick plate and demanding applications. Density for weight calculation is 7.85 g/cm3 (7850 kg/m3) for all of these carbon steels. When ordering, buyers should state the standard edition, quality grade, thickness tolerance class and delivery condition, because the same nominal grade can behave differently in a 6 mm sheet and a 60 mm plate.
Selection Guidance for Shipbuilding, Construction and Wear Applications
For ship hull structure and marine equipment, Q355C/D/E or A572 Gr.50 with a Charpy impact requirement matched to the service temperature is the normal choice, and the P/S limits of the higher grades matter more than the nominal yield. For building frames, cranes and transmission towers, Q355B or A572 Gr.50 delivered hot-rolled is usually sufficient. Where abrasion is the main risk, the base plate should be specified with a higher hardness or supplied with a wear-resistant surface treatment rather than relying on the structural grade alone. In every case, the supplier should provide the mill test certificate showing heat number, chemical analysis and mechanical test results so the delivered material can be traced to its production heat.
Frequently Asked Questions
Is Q355 the same steel as ASTM A572 Gr.50?
They are at the same strength level (355 vs 345 MPa minimum yield) but are defined by different standards with different chemistry limits, tolerances and testing rules. They are equivalent in many designs, but substitution should be confirmed by the project engineer using the mill certificate data.
What does the letter B in Q355B mean?
It is the quality grade. Grade B controls phosphorus and sulphur to 0.035% max but sets no mandatory low-temperature impact test; Grades C, D and E add impact requirements of 34 J at 0, -20 and -40 degrees C respectively.
What is the density of Q355 steel for weight calculation?
7.85 g/cm3, the same as other structural carbon steels. A 10 mm thick plate weighs about 78.5 kg per square metre.
Why does the yield strength drop when the plate is thicker?
Thicker plates receive less rolling reduction and cool more slowly, producing a coarser structure with lower strength per unit area. The standard property tables account for this with thickness-dependent minimum values.
Can Q355 be welded to A36 or S235JR steel?
Yes. Matching or lower-strength filler metal and a qualified welding procedure are required, with preheat considered for thick sections and cold-weather work. The joint design should follow the requirements of the governing standard.
What should the mill test certificate contain?
A complete certificate states the standard and edition, grade, heat number, chemical analysis, tensile and impact results, and the delivery condition, allowing the buyer to verify that the material actually meets the ordered specification.