Galvanized rectangular tubes can be welded, but the zinc coating makes the process different from welding plain carbon steel tube. Zinc melts at about 419 degrees Celsius while steel melts at about 1538 degrees Celsius, so during welding the zinc layer vaporizes long before the steel melts. If this is not managed, the weld suffers porosity and cracking, the operator breathes zinc oxide fume, and the coating around the joint is destroyed. This article covers the core problems, the safety rules, joint preparation, process selection and post-weld corrosion protection, following the repair guidance of ISO 1461 and the welding practice of EN 1011.
How the Zinc Layer Affects the Weld
| Effect | Cause | Consequence |
|---|---|---|
| Porosity | Zinc vapor is trapped in the solidifying weld metal | Reduced weld density and load capacity |
| Zinc embrittlement | Molten zinc penetrates the weld grain boundaries | Lowered toughness, risk of cracking under stress |
| Coating burn-off | Heat destroys zinc over roughly 50-100 mm around the weld | Exposed steel rusts unless re-protected |
| Zinc fume | Zinc vapor oxidizes to zinc oxide fume | Metal fume fever if inhaled over long periods |
The vaporized zinc also changes the weld bead shape: droplets of zinc on the joint surface can cause spatter and an uneven root, so joints welded without preparation usually look worse and test worse than the same joint welded on bare steel.
Safety First: Zinc Fume Control
The immediate hazard of welding galvanized tube is zinc oxide fume. Inhaled in sufficient quantity it causes metal fume fever, with symptoms of fever, chills and coughing that appear several hours after exposure. Control measures are mandatory: weld in a well-ventilated area or use local exhaust extraction, wear a suitable respirator with particulate protection, and never weld galvanized tube in a confined space without forced ventilation and monitoring. These are not optional extras; they protect the welder on every joint.
Preparing the Joint
The most reliable way to avoid porosity and zinc embrittlement is to remove the zinc coating from the weld zone before welding. Grind or abrade the coating off the joint faces and the surrounding area, typically 25 to 50 mm on each side of the joint, until bare steel is visible. This eliminates the source of zinc vapor at the weld, so the weld metal solidifies dense and sound. The removed coating must be restored afterwards, which is why preparation and repair are planned as one operation. Where the design allows, mechanical fastening with sealed joints or adhesive bonding can avoid welding altogether, but where welding is required, preparation is the key step.
Selecting the Welding Process
For thin-wall galvanized rectangular tube, the practical choices are gas metal arc welding (MIG/MAG) and gas tungsten arc welding (TIG), both of which concentrate heat and allow good control. Resistance spot welding and seam welding also work well on the tube wall when the zinc layer is thin, because the very short weld time limits zinc vapor formation. Oxy-fuel welding should be avoided for galvanized tube: the slow, broad heat input burns a large area of coating and produces heavy fume. Whatever the process, use a technique that keeps the arc as short as possible, direct the heat to the joint, and let the welder work at a consistent travel speed so the heat-affected zone stays small.
Restoring Corrosion Protection After Welding
Welding removes the zinc coating over roughly 50 to 100 mm around the joint, so the weld area must be re-protected or the structure will rust at the weld within months. The standard repair method is cleaning the affected area to bright metal, then applying a zinc-rich paint or spray in multiple coats to build a dry film thickness equivalent to the original galvanized coating; this is the field-repair route accepted in ISO 1461 for damaged coatings. For larger damaged areas or joints that will see severe service, thermal spray zinc (metal spraying) or a full re-galvanizing dip for small fabricated parts gives a thicker, metallurgically bonded layer. In every case, the repair coating must cover the weld and the full burn-off zone, and its thickness should be checked before the part goes into service.
FAQ
Is it safe to weld galvanized rectangular tube?
Yes, when fume is controlled: weld with good ventilation or local extraction and wear a suitable respirator, because zinc oxide fume can cause metal fume fever.
Why do welds on galvanized tube contain pores?
The zinc coating vaporizes in the arc and the gas is trapped in the solidifying weld metal. Removing the zinc from the joint area before welding is the effective cure.
Should the zinc coating be removed before welding?
Yes. Grind the coating off the joint faces and 25-50 mm each side so the weld metal is dense and free of zinc porosity and embrittlement.
How much coating is lost around a weld?
The heat burns the zinc over roughly 50-100 mm around the joint. That area must be cleaned and re-protected with zinc-rich paint or thermal spray zinc.
Can the tube be re-galvanized after welding?
Small fabrications can be hot-dip re-galvanized to ISO 1461. For large structures where re-dipping is impractical, repair the damaged coating with zinc-rich paint or metal spray.
Is the weld strength of galvanized tube lower than plain tube?
No, provided the zinc is removed at the joint and the weld is sound. The weld strength is governed by the base metal and the weld procedure, not by the coating.