Cold rolled steel surface cleaning

Aug 20, 2025 Leave a message

1.What are the common pollutants and hazards on the surface of cold-rolled steel?

Oil contamination: This primarily comes from rolling oil (used for lubrication and cooling, containing mineral oil, emulsifiers, etc.) during the rolling process, equipment lubricant leaks, or volatile oil residue from annealing. If not removed, this can lead to poor adhesion of the paint/plating during subsequent coating (bubbles and flaking), or mold slippage and workpiece damage during stamping.
Oil scale/rust: This often occurs after non-bright annealing (annealing without air isolation, resulting in the formation of oxide layers such as Fe₂O₃ and Fe₃O₄ on the surface) or minor rust caused by improper storage. Oxide scale can roughen the surface, leading to uneven coating coverage and the possibility of flaking and scratching the sheet during processing.
Solid impurities: These include iron powder and metal debris left over from rolling, as well as dust and particulate matter from storage/transportation. These impurities can cause pinholes and bumps on the coated surface, or damage the sheet surface during stamping. Pickling residue: If the rinse after pickling is not thorough, acid (such as hydrochloric acid) or salts (such as FeCl₂) may remain on the surface, which will accelerate the corrosion of the plate (yellow spots and rust spots).

Cold rolled coil

2.What are the commonly used chemical cleaning agents and their applicable scenarios?

Alkaline cleaners contain sodium hydroxide, sodium carbonate, sodium silicate, and surfactants (such as sodium alkylbenzene sulfonate). They remove oil stains through alkaline hydrolysis (oil forms soluble soaps under alkaline conditions) and emulsification and dispersion (surfactants reduce the adhesion of oil stains to the sheet material, causing the oil to form small droplets suspended in water). They are suitable for mineral oil stains such as rolling oil and lubricating oil, and are mildly corrosive to sheet materials (alkaline concentration must be controlled to avoid excessive corrosion).
Acidic cleaners primarily use hydrochloric acid, sulfuric acid (at low concentrations), or citric acid (an organic acid). They are effective against mill scale and rust stains. The acid reacts with the mill scale to form soluble salts (such as FeCl₂ and FeSO₄), which are removed with the solution. Acid cleaning is often combined with alkaline cleaning (first using acid to remove scale, then alkaline to remove oil). However, it's important to note that cold-rolled steel is mostly low-carbon steel. Excessive acid concentrations (e.g., hydrochloric acid concentrations > 20%) or high temperatures (> 60°C) can corrode the substrate, resulting in surface roughness. (Corrosion inhibitors, such as hexamine, are required to reduce the corrosion rate.)
Neutral cleaning agents, primarily based on surfactants (such as nonionic surfactants), have a pH of approximately 7 and remove light oil and dust through emulsification and penetration. They are suitable for cold-rolled steel requiring extremely high surface finishes (such as those used in precision instruments), avoiding acid and alkali corrosion.

Cold rolled coil

3.What are the commonly used cleaning processes?

Immersion: Cold-rolled sheet (or sheet unwound from a coil) is immersed in a chemical solution (heated to 40-60°C to accelerate the reaction), combined with stirring or ultrasonic waves (high-frequency vibrations to remove contaminants). Suitable for small batches of complex-shaped sheets, this method requires simple equipment but is less efficient.
Spray: A high-pressure spray nozzle (0.2-0.5 MPa) sprays the chemical solution onto the sheet surface, using both impact force and chemical action to remove contaminants. Suitable for continuous production lines (such as cold-rolled sheet finishing lines), this method offers high efficiency (speeds of up to 10-30 m/min) and can be combined with a roller brush for enhanced results.

Cold rolled coil

4.What are the common methods of physical cleaning?

Roller Brush Cleaning: Brush rollers (made of nylon or bristle, selected based on the surface finish of the plate-soft nylon for precision plates, hard bristle for rough plates) are installed on the cleaning line. As the plate passes, the brush rollers rotate (at a speed of 100-300 rpm), rubbing against the surface to remove iron powder, dust, and emulsified oil. Brush pressure must be controlled (usually 0.1-0.3 MPa). Excessive pressure can scratch the plate surface (especially bright cold-rolled plate).

High-Pressure Water Flushing: High-pressure water (0.5-1.0 MPa) is sprayed onto the plate surface. This is primarily used to remove chemical residues (such as acid after pickling and alkali after alkaline washing) and contaminants loosened by chemicals. The water temperature (room temperature or 40-50°C for optimal flushing) and the water flow angle (at a 30-45° angle to the plate surface to prevent rebound and secondary contamination) must be controlled. Ultrasonic cleaning: Ultrasonic waves (20-40kHz frequency) are introduced into the cleaning tank, generating numerous tiny bubbles in the liquid. When these bubbles burst, they generate localized high pressure, impacting contaminants trapped in crevices on the plate surface (such as oil stains and iron dust in narrow corners). This method is suitable for precision cold-rolled plate (such as those used in electronic components) or complex structural parts, achieving high cleaning precision (removing even micron-sized impurities).

 

5.How to control the key parameters of the cleaning process?

Chemical Concentration: Alkaline cleaning agents typically have a concentration of 2-5% (higher concentrations can easily leave residue, while lower concentrations can result in insufficient cleaning power); acidic cleaning agents (hydrochloric acid) have a concentration of 5-15% (use a corrosion inhibitor to keep the corrosion rate below 0.1g/m²·h).
Temperature: Higher temperatures accelerate the reaction of the cleaning agents (e.g., alkaline cleaning temperatures of 40-60°C increase oil emulsification efficiency by 30%), but avoid excessive temperatures (e.g., temperatures exceeding 80°C can cause surfactant decomposition and render the cleaning agent ineffective).
Cleaning Time: Spray cleaning requires a line speed of 10-30m/min (pass time of 10-30 seconds), while immersion cleaning requires 3-10 minutes (adjusted depending on the thickness of the contaminant). Too short a time will result in incomplete cleaning, while too long a time may cause excessive corrosion on the panel surface. Mechanical strength: brush roller pressure 0.1-0.3MPa, high-pressure water pressure 0.3-1.0MPa (use lower pressure for bright boards to avoid scratches; use higher pressure for rough boards to improve peeling effect).