DC04 and DC05 Are Cold Rolled Carbon Steel Grades, Not Stainless Steel
DC04 and DC05 belong to the cold rolled low carbon steel family defined by EN 10130. They are aluminium-killed, non-alloy steels supplied as coil, slit strip, cut sheet or blank, and they are selected for one characteristic above all others: the capacity to be drawn into deep, complex shapes without splitting. Neither grade carries a chromium addition, so neither is a stainless steel. Where corrosion resistance is required, the practical routes are a hot-dip zinc coating, a 55% aluminium-zinc coating, or a genuinely stainless substrate instead of the DC family.
The DC ladder starts at DC01 for commercial-quality bending and shallow forming, continues through DC03 and DC04 for general deep drawing, and reaches DC05, DC06 and DC07 for progressively more severe drawing. Each step up the ladder buys formability by making the microstructure cleaner, softer and more favourably textured, which is why yield strength falls while the plastic strain ratio and the work hardening exponent rise.
Grades, Standards and Typical Supply Forms
DC04 also carries the European material number 1.0338, DC05 is 1.0312 and DC06 is 1.0873. EN 10130 specifies cold rolled low carbon flat products for cold forming, EN 10131 covers dimensional and shape tolerances, GB/T 5213 is the Chinese specification for cold rolled sheet for cold forming, and JIS G 3141 covers the SPCC, SPCD and SPCE series that many Asian drawings cite alongside the DC grades.
| Grade | Material number | Forming duty | Usual supply form |
|---|---|---|---|
| DC01 | 1.0330 | Commercial quality, bending and shallow forming | Coil, sheet |
| DC03 | 1.0347 | Drawing quality, moderate profiling | Coil, slit strip, sheet |
| DC04 | 1.0338 | Deep drawing quality | Coil, slit strip, blank |
| DC05 | 1.0312 | Higher deep drawing quality | Coil, slit strip, blank |
| DC06 | 1.0873 | Ultra deep drawing quality | Coil, slit strip, blank |
Chemical Composition and Why It Matters
Composition for the drawing grades is engineered around three ideas: hold carbon low so the ferrite stays soft, hold phosphorus and sulphur low so that inclusions and solid-solution hardening cannot open a crack, and add aluminium or micro-alloying elements such as titanium and niobium to fix the residual carbon and nitrogen atoms that would otherwise cause ageing and stretcher strain. The table below gives the typical maximum values applied to the grades most frequently ordered in coil and strip form.
| Grade | C max % | Mn max % | P max % | S max % | Al min % | Ti + Nb max % |
|---|---|---|---|---|---|---|
| DC04 | 0.08 | 0.40 | 0.025 | 0.025 | 0.015 | - |
| DC05 | 0.06 | 0.35 | 0.020 | 0.020 | 0.015 | - |
| DC06 | 0.03 | 0.30 | 0.020 | 0.020 | 0.015 | 0.20 |
Mechanical Properties and Formability Indicators
Two indicators separate a deep drawing grade from an ordinary cold rolled grade. The plastic strain ratio r90 describes how the sheet resists thinning when it is stretched; the work hardening exponent n90 describes how the material distributes strain before local necking starts. Higher values of both mean a deeper, safer draw. Elongation rises with thickness, so the values below are quoted for annealed and skin-passed material in the usual thickness window and are intended for grade comparison; the agreed order specification governs each delivery.
| Grade | Yield strength Re (MPa) | Tensile strength Rm (MPa) | Elongation A80 (%) | r90 | n90 |
|---|---|---|---|---|---|
| DC04 | 210 max | 270 - 350 | 36 min | 1.6 min | 0.18 min |
| DC05 | 180 max | 270 - 350 | 38 min | 1.9 min | 0.20 min |
| DC06 | 100 - 180 | 270 - 370 | 39 min | 2.0 min | 0.22 min |
Surface Finish, Tolerances and Forming Guidance
Cold rolled DC04 and DC05 strip is normally delivered with a matte or bright finish and a light skin pass, which suppresses the yield-point elongation that would otherwise show up as orange-peel marks across a drawn panel. Thickness, width, camber, flatness and edge condition follow EN 10131 unless a tighter agreed tolerance is ordered. Coil is supplied on 508 mm or 610 mm inner diameter bores and can be slit to the customer width, oscillate wound, or cut into sheets and blanks so that the press shop receives material matched to its blanking layout.
Draw radii should be generous relative to sheet thickness, and the die clearance kept tight to control the wall thickness of the drawn wall.
Adequate lubrication matters more than press tonnage: DC04 and DC05 tolerate a lower blank-holder force because their texture carries strain into the flange instead of the wall.
Both grades weld readily by spot, seam and laser processes; the very low carbon content keeps the weld zone soft and limits hardness peaks.
Store coil indoors and dry, with the eye horizontal, to keep the surface free from condensation staining before forming and painting.
Frequently Asked Questions
Q: Are DC04 and DC05 stainless steel?
No. They are unalloyed low carbon cold rolled steels defined by EN 10130 and contain no chromium addition. Their corrosion protection comes from a coating or a paint system, not from the substrate chemistry.
Q: What is the difference between DC03, DC04 and DC05?
DC03 suits moderate profiling and ordinary deep drawing, DC04 handles high forming requirements such as deep drawn housings, and DC05 is chosen when the draw is deeper still or the flange must be stretched further before it tears.
Q: Why do the quoted elongation values change with thickness?
The uniform elongation of a soft, textured ferritic sheet increases as the section becomes thicker, so a 1.5 mm coil shows a higher A80 figure than a 0.5 mm coil of the same grade.
Q: Can DC04 be supplied with a coating?
Yes. The cold rolled substrate is regularly used as the base for hot-dip zinc, zinc-iron or 55% aluminium-zinc coatings, and the resulting coated product is specified under its own coating standard rather than under EN 10130 alone.
Q: Is DC04 the same as 1.0338?
Yes. 1.0338 is the European material number for the DC04 grade, and drawings from different regions frequently use one identifier or the other for the same steel.
Q: How should a press shop handle stretcher strain?
Order skin-passed material, keep the coil in a controlled store, and avoid long dwell periods between the last forming operation and painting so that the sheet cannot age back into a condition that produces Lüders bands.