Hot-rolled carbon steel plate in grades Q195, Q215, Q235, Q345 and Q355 is the most widely used structural steel family in Chinese manufacturing and construction. It is strong enough for a huge range of frames, tanks, machines and building structures, and inexpensive compared with alloy or stainless steel. What buyers often forget is that these are plain carbon steels: they corrode in humid air, and the service life of the finished structure depends on the corrosion protection system applied after fabrication.
Understanding the Grade Names
The letter Q stands for yield strength in Chinese steel standards, and the number is the guaranteed minimum yield strength in megapascals for the thin thickness range. Q195 and Q215 are lower-strength structural grades defined in GB/T 700; Q235 is the most common general structural grade in the same standard; Q345 is the classic low-alloy high-strength grade formerly defined in GB/T 1591; and Q355 is its successor in the current GB/T 1591, with a slightly adjusted specification. The suffix letters B, C and D indicate guaranteed impact toughness at different temperatures: B means 20 degrees Celsius, C means 0 degrees, and D means minus 20 degrees. Q235B and Q355B are therefore the standard options for ordinary outdoor and indoor structures.
Mechanical Properties at a Glance
The guaranteed properties below follow GB/T 700 and GB/T 1591 for plates up to 16 millimetres thick, the range most commonly used in general fabrication.
| Grade | Standard | Yield strength Re | Tensile strength Rm | Elongation |
|---|---|---|---|---|
| Q195 | GB/T 700 | 195 MPa min | 315 to 430 MPa | 33% min |
| Q215 | GB/T 700 | 215 MPa min | 335 to 450 MPa | 31% min |
| Q235 | GB/T 700 | 235 MPa min | 370 to 500 MPa | 26% min |
| Q345 | GB/T 1591 (superseded) | 345 MPa min | 470 to 630 MPa | 22% min |
| Q355 | GB/T 1591 | 355 MPa min | 470 to 630 MPa | 22% min |
Does Q235 Rust? Corrosion Behaviour Explained
Yes, Q235 rusts. Its resistance to atmospheric corrosion is average: in dry indoor air it corrodes slowly, but in humid environments, coastal atmospheres or contact with water, rust forms quickly. The mechanism is electrochemical: moisture on the surface dissolves oxygen, iron dissolves at anodic areas and rust precipitates. Q235 contains no significant chromium, nickel or copper addition, so it has none of the self-passivating behaviour of stainless steel or the oxide stabilisation of weathering steel. This is not a defect of the grade, but it means the specification must always include a protection plan.
Common Corrosion Protection Methods for Q235 and Q355
Painting systems
For outdoor structures, the classic system is epoxy zinc-rich primer plus epoxy intermediate and polyurethane or acrylic topcoat, selected according to ISO 12944 and the corrosivity category of the site. The zinc-rich primer protects the steel sacrificially at scratches and cut edges, while the topcoat provides colour and UV resistance.
Hot-dip galvanizing
Q235 and Q355 can both be hot-dip galvanized, and this is the most common way to improve corrosion resistance economically. The zinc coating protects the steel by barrier effect and by sacrificial action, and typical coating masses for structural work follow ISO 1461, commonly 70 to 85 micrometres for thick plate sections. Galvanized parts are then often painted in a duplex system for a much longer service life.
Powder coating and passivation
Powder coating gives a thick, tough film for indoor and semi-outdoor products such as cabinets and racks. Passivation and film-forming oils give only short-term protection between processes. Pickling or sandblasting before these treatments removes mill scale and oil, and creates the anchor profile needed for adhesion.
Purpose of Pickling and Sandblasting
Hot-rolled plate leaves the mill with a layer of black oxide scale. Pickling dissolves this scale with acid, usually hydrochloric acid, leaving a clean grey surface; sandblasting or shot blasting removes scale and rust mechanically and produces a uniform anchor profile. Both operations prepare the steel for painting, galvanizing or welding, and both are also used before surface inspection to reveal defects. For galvanizing, sandblasting is often preferred where the surface must be uniformly active for a good zinc reaction.
How to Distinguish Q235 from Stainless Steel on Site
The quickest field test is a magnet plus a look at the surface. Q235 is strongly magnetic and develops brown rust within days or weeks outdoors, while 304 stainless steel is only weakly magnetic, if at all, and stays bright. A grinding test also works: Q235 throws bright sparks and rusts where ground, while stainless steel grinds with a duller, redder spark and stays clean. For a definitive answer, a mill certificate or a chemical analysis per GB/T 700 or ASTM A751 is required.
Frequently Asked Questions
Q1. Which Q-grade should I choose for a welded frame?
For most general frames, Q235B is the economical default. When the design needs higher strength to save weight, for example in long-span or heavy-load structures, Q355B is the standard upgrade and welds with similar processes.
Q2. Can Q235 be galvanized without problems?
Yes. Hot-dip galvanizing is the most common method to improve the corrosion resistance of Q235. Pickle or sandblast first to remove scale, and confirm the silicon content is suitable for a uniform zinc layer.
Q3. Is Q355 the same steel as Q345?
Not exactly. Q355 is the successor grade in the current GB/T 1591, with a slightly adjusted composition and a nominal yield of 355 MPa instead of 345 MPa. Many mills supply Q355 where Q345 was previously ordered, and certificates should state the applicable standard version.
Q4. How long does Q235 last outdoors without protection?
It depends on the environment. In a mild dry climate, light surface rust appears within weeks but section loss is slow; in a humid coastal or industrial atmosphere, significant corrosion can develop within a few years. Unprotected carbon steel is never a long-term outdoor solution.
Q5. What is the best protection for a Q235 structure near the sea?
Use a duplex system: hot-dip galvanizing per ISO 1461 followed by a paint system designed for the marine corrosivity category C5-M per ISO 12944. Pay special attention to cut edges, welds and bolted connections.
Q6. How do I know the real yield strength of delivered Q235 plate?
Ask for the mill test certificate, which states the heat number, chemical analysis and mechanical test results per GB/T 700. For critical projects, take samples and test yield, tensile and elongation in an independent laboratory.