How do you determine the yield strength of cold-rolled coils?

Feb 12, 2026 Leave a message

1.What are the three pitfalls you absolutely must be aware of?

The unit is MPa, not kgf/mm². Older drawings often use "35 kgf/mm²", where 1 kgf/mm² ≈ 9.8 MPa. 35 kgf ≈ 343 MPa. Confusing these units will lead to selecting the wrong material.

Transverse vs. Longitudinal Strength: The longitudinal strength of cold-rolled coils is usually lower than the transverse strength.

Deep-drawn parts (drawing): Look at the transverse direction; transverse strength determines whether it will crack.

Rolled parts (roll forming): Look at the longitudinal direction.

If the warranty certificate doesn't specify the direction, it defaults to longitudinal; don't blame the steel mill if it cracks during stamping.

Tolerance Range: The national standard allows a deviation of ±(20~30) MPa. Buying DC03 (≤240 MPa), with an actual test value of 265 MPa, is compliant but not necessarily usable-it will definitely crack when stamping complex deep-drawn parts.

cold-rolled coil

2.How to test the bending method with one hand?

<180MPa (Extremely Soft): Bending 90° by hand, it has no springback, like lead.

180~240MPa (Soft): Bending 90°, it springs back 10~20° upon release.

240~300MPa (Semi-Hard): Requires force, springs back at a large angle, and causes hand fatigue.

>300MPa (Hard): Very difficult to bend by hand, and basically springs straight back upon release.

cold-rolled coil

3.How about pinching the edge of the nail?

Try pinching the cut surface (burr edge) of the steel strip with your fingernail.

Soft material: Your fingernail can leave a shallow mark, or even curl off metal shavings.

Hard material: Your fingernail will slip, leaving no mark.

cold-rolled coil

4.What are the effects of excessively high yield strength?

Insufficient annealing: The bell-type furnace did not heat thoroughly, resulting in insufficient core temperature.

→ Symptoms: Soft at the beginning and end, hard in the middle; or soft at the edges, hard in the core.

Excessive elongation during leveling: The leveling machine applied too much pressure, causing work hardening.

→ Symptoms: The elongation is uniformly high throughout the coil, with a slightly rough surface.

Mixing materials: Low-carbon steel was mixed with high-strength steel.

→ Symptoms: Sudden change in hardness, with a difference of more than 50 MPa within the same coil.

 

5.What are the effects of having too low a yield strength?

Over-annealing: Too high a temperature or too long a holding time results in coarse grains.

→ Symptoms: Darkened surface, even orange peel texture.

Unevenness: Insufficient leveling machine or too low elongation.

→ Symptoms: Loose winding, warped sheet shape, yield plateau (Lüders band) during stretching.