How to ensure the continuity of the coating on S235JR galvanized products?
Ensuring the continuity of the coating on S235JR galvanized products (i.e., the zinc layer completely covers the substrate, free of defects such as missing plating and pinholes) is crucial to ensuring its corrosion resistance. This requires strict control at multiple stages, including substrate pretreatment, galvanizing process control, and equipment maintenance. Specific measures are as follows:
1. Substrate Pretreatment: Remove surface impurities to ensure the adhesion of the zinc layer.
S235JR is a low-carbon steel, and its surface is susceptible to impurities such as scale, rust, oil, and welding slag. These impurities can hinder contact between the zinc solution and the substrate, leading to missing plating. Pretreatment requires the following:
Degreasing
Use alkaline cleaning (such as sodium hydroxide solution), pickling (hydrochloric acid or sulfuric acid), or ultrasonic cleaning to thoroughly remove rolling oil, cutting oil, fingerprints, and other oils from the substrate surface. Residual oil can form "oil spots," preventing the zinc layer from adhering and resulting in missing plating points.
After cleaning, rinse with clean water to prevent residual acid or alkali from corroding the substrate or affecting subsequent processing. Rust and Scale Removal
S235JR hot-rolled steel often has scale (Fe₃O₄, FeO, etc.) on its surface, which requires removal through pickling (primarily hydrochloric acid, 15%-20% concentration) or mechanical rust removal (such as sandblasting or shot blasting). Incomplete scale removal prevents the zinc solution from reacting with the base iron, resulting in "black spots" or plating gaps.
After pickling, an "activation" treatment (such as a dilute acid dip) is required to remove residual oxidation products, exposing the fresh iron substrate and ensuring metallurgical bonding of the zinc layer.
Repairing Base Defects
Inspect the base material surface for mechanical defects such as cracks, folds, and pits. These areas can easily accumulate impurities, preventing the zinc solution from filling during galvanizing, resulting in localized plating gaps. Pre-grinding or repairing is recommended to ensure a smooth surface. II. Hot-Dip Galvanizing Process Parameter Control: Ensure Uniform Coverage with the Galvanizing Solution
Hot-dip galvanizing (continuous or batch galvanizing) is the most commonly used galvanizing method for S235JR. Process parameters directly affect the continuity of the zinc coating:
Zinc Solution Composition and Temperature
Zinc Solution Purity: Impurities such as lead, tin, and aluminum must be controlled (excessive aluminum content may reduce zinc coating adhesion, while excessively low content may affect zinc spangle morphology). This prevents impurities from forming "zinc slag" that adheres to the substrate surface, resulting in areas without a zinc coating.
Temperature Control: The zinc solution temperature is typically between 440-460°C (for mild steel). Excessively high temperatures reduce the fluidity of the zinc solution, easily leading to the formation of zinc nodules. Excessively low temperatures increase the viscosity of the zinc solution, making it difficult to evenly coat complex structures (such as corners and grooves), potentially resulting in missed coatings.
Zinc Dipping Time and Speed: The dipping time should be adjusted based on the substrate thickness (usually 1-3 minutes) to ensure that the zinc solution fully penetrates the substrate surface, especially in areas with no smears such as weld seams and perforations. Too short a time may result in the alloy layer failing to form in some areas, while too long a time may result in a thick zinc coating that is prone to flaking. The workpiece must be placed in and out of the zinc bath at a steady speed to avoid violent shaking that could cause splashing and localized "iron exposure."
Flux Treatment
Pretreated workpieces should be dipped in a flux (such as a zinc chloride-ammonium chloride solution) to form a protective film. This prevents secondary oxidation of the substrate before entering the zinc bath and promotes the reaction between the zinc bath and the substrate. The flux concentration and temperature (usually 60-80°C) must be stable, otherwise "hard plating" (weak zinc adhesion or partial loss of zinc coating) can easily occur.
III. Post-Processing and Quality Inspection: Promptly Detect and Repair Defects
Cooling and Passivation
After removal from the zinc bath, the workpiece should be cooled slowly (to avoid cracking of the zinc layer caused by rapid cooling). After cooling, a passivation treatment (such as chromate or chromium-free passivation) can be used to form a protective film on the zinc surface, masking tiny pinholes and enhancing corrosion resistance. Strict Quality Inspection
Appearance Inspection: Visually or with the aid of a magnifying glass, inspect the surface for defects such as missing plating (exposed iron spots), pinholes (tiny holes), and localized zinc coating defects caused by zinc nodules. Focus on areas prone to missing plating, such as corners, welds, and grooves.
Coating Continuity Test: For key products, an "adhesion test" (such as a bend test, where the zinc layer is bent 180° to observe whether cracks or exposed iron appear) or a "copper sulfate test" (where the zinc layer dissolves over time to determine if missing plating is present) can be performed.
If missing plating defects are discovered, sandpaper should be used to polish the missing areas to expose fresh substrate. Local repairs can then be performed using cold zinc spraying, touch-up paint, or other methods to ensure overall continuity.
IV. Equipment Maintenance and Environmental Control
The zinc slag at the bottom of the galvanizing tank should be regularly cleaned to prevent it from adhering to the workpiece surface and forming "slag spots" (resulting in localized zinc coating defects).
The conveyor equipment on the production line (such as rollers and hooks) should be kept clean to prevent oil or impurities from contaminating the workpiece surface.
The solutions in the pretreatment tanks (degreasing, pickling, and fluxing) should be replaced regularly to prevent impurities from accumulating and affecting the treatment results.