DC02 is a continuously annealed, aluminium-killed low carbon cold rolled steel supplied under EN 10130, with the same DC02 designation available in the GB/T 5213 series. It sits one step above the basic commercial grade DC01 and one step below the drawing grades DC03 and DC04, which is precisely why it has become the default substrate for shallow drawing, bending, flanging and blanking of appliance housings, brackets, mounting plates and automotive interior panels.
The grade is not selected on price alone. It is selected because moderate yield strength combined with a wide plastic range and high elongation keeps springback, thinning and edge cracking predictable across long, high-volume press runs, so die tryout time and scrap rate both stay low.
Composition and Mechanical Property Targets
Stamping behaviour begins with the ladle analysis. DC02 is normally supplied fully killed and aluminium treated, with a fine and uniform grain structure so that thinning is distributed evenly across the blank instead of concentrating in one weak area.
| Element | Typical ladle analysis (%) | Effect on stamping |
|---|---|---|
| C | 0.10 max | Higher carbon raises strength and cuts elongation |
| Mn | 0.45 max | Controls strength without harming ductility |
| P | 0.035 max | Excess phosphorus embrittles the bend line |
| S | 0.035 max | Sulphide inclusions initiate edge cracks |
| Al | 0.020 min | Fully killed, fine grain, stable ageing behaviour |
The mechanical property window is the practical control point for press shop engineers, because it defines how much the blank can stretch before it tears and how much it springs back after the punch releases.
| Cold rolled grade | Typical yield strength Re (MPa) | Minimum elongation A80 (%) | Best-fit process |
|---|---|---|---|
| DC01 | 280 max | 28 | General forming, simple bends |
| DC02 | 140 to 240 | 34 | Shallow drawing, bending, blanking |
| DC03 | 120 to 210 | 36 | Moderate drawing |
| DC04 | 110 to 190 | 38 | Deep drawing, complex geometry |
In practice, a low yield strength gives good stretchability but can produce wrinkling in unsupported areas, while a high yield strength demands greater press tonnage and increases the risk of cracking at tight radii. The DC02 range is deliberately centred so that most shallow punch-and-bend duties fall inside a comfortable window. A tensile strength roughly 130 MPa above yield point confirms that there is enough plastic reserve for the material to redistribute local stress concentrations instead of fracturing at the first peak.
Formability Behaviour Under the Press
Springback: because Re is moderate rather than high, springback after bending stays small and can usually be absorbed with a slight die angle compensation instead of an additional restrike station.
Stretch and flanging: high elongation lets the sheet follow flared, curved and flanged features without splitting, which suits refrigerator liners, microwave shells, control panels and automotive interior trim.
Bending: crack-free results are achievable at a full 180 degree bend with a bend core diameter of only about 0.5 times the sheet thickness, which supports the tight right-angle and curved returns used in appliance cabinets.
Strain distribution: uniform grain size keeps stretcher strains and orange-peel defects away from visible Class A surfaces.
Blanking, Shearing and Edge Quality
In the separation process, DC02 behaves predictably as long as clearance is set correctly and tooling is kept sharp.
| Parameter | Recommended setting | Comment |
|---|---|---|
| Punch-die clearance | 8 to 12 percent of sheet thickness | For 1.0 mm sheet, 0.08 to 0.12 mm |
| Burr height target | 0.1 times sheet thickness or less | Blunt edges push burrs above this limit |
| Punching speed | 100 to 200 strokes per minute on conventional presses | Suits heat dissipation holes and mounting holes |
| Thickness for high-speed blanking | 3.0 mm and below | Above 4 mm, reduce speed to prevent edge chipping |
Low deformation resistance means die wear is modest and tool life is long. Tooling that is correctly ground also keeps the sheared cross-section smooth and reduces the secondary deburring operation, which matters when the blank feeds straight into a welding or painting line.
Die Design and Lubrication Settings
Die geometry decides whether the material flows or fails. The following settings are the usual starting point for DC02 tooling and are then trimmed during tryout.
| Die element | Recommended value | Failure mode if ignored |
|---|---|---|
| Drawing die clearance | 1.1 to 1.2 times sheet thickness | Excessive extrusion and wall thinning |
| Punch radius, convex R | 2 times sheet thickness or greater | Local overstretching and splits |
| Die radius, concave R | 3 times sheet thickness or greater | Wrinkling and restricted material flow |
| Lubricant | Stamping emulsion with 5 to 10 percent oil content | Scoring, pick-up and surface cracking |
For a 1.0 mm workpiece this means a punch radius of at least 2 mm and a die radius of at least 3 mm. Straight motor oil should not be used as a press lubricant because it leaves heavy residue that interferes with subsequent phosphating and painting. When tooling radii cannot be increased, moving one grade up to DC03 or DC04 is more economical than repeatedly adjusting the press.
Incoming Material Control and Process Optimisation
Surface condition: specify surface grade FB or FC where visible parts are produced. Scratches, scale and oil stains act as stress raisers and cause cracking or wrinkling, so blanks are wiped with alcohol before forming.
Thickness consistency: the standard thickness tolerance for DC02 sheet is around plus or minus 0.05 mm. Keep the variation inside one batch within plus or minus 0.03 mm to avoid uneven deformation and inconsistent springback.
Property uniformity: require a coil-by-coil mechanical property report and hold yield strength variation along one coil to 20 MPa or less. Larger swings, for example 240 MPa at the head against 140 MPa at the tail, translate directly into inconsistent part geometry.
Pre-treatment: for sheet thicker than 3 mm, a stress relief anneal at 250 to 300 degrees Celsius for one hour restores some plasticity and can add 2 to 3 percentage points of elongation.
Tooling upkeep: polish cutting edges and forming surfaces about every 10,000 strokes to remove pick-up before it scratches the workpiece.
Part inspection: concentrate on the drawn bottom and bent radii, use dye penetrant for micro-crack detection and verify that thickness reduction stays within 15 percent.
Process matching matters more than any single parameter. For shallow punching and bending, DC02 gives the best cost-to-performance balance. For genuinely deep drawn components such as fuel tanks or washing machine drums, specify DC04 or DC05 from the start rather than accepting the scrap rate that a mismatched commercial grade will generate.
Frequently Asked Questions
Q: Can DC02 replace DC01 without changing the tooling?
In most shallow bending and blanking duties yes, because DC02 is softer and more ductile than DC01 and can run in the same die. Expect slightly less springback, so a small press adjustment is usually all that is needed.
Q: What clearance should be used when blanking 1.0 mm DC02 sheet?
Set punch-die clearance at 8 to 12 percent of the sheet thickness, which is 0.08 to 0.12 mm per side, to keep burrs below roughly 0.1 times the sheet thickness.
Q: Why do parts crack at the radius even though the grade is ductile?
Typical causes are a punch radius below twice the sheet thickness, an under-lubricated die, or surface scratches acting as stress raisers. Increase the radius, switch to a stamping emulsion and check incoming surface quality.
Q: How much yield strength variation inside one coil is acceptable?
Hold the variation to about 20 MPa. A wider spread produces visible differences in springback between parts formed from the head and the tail of the same coil.
Q: Is DC02 suitable for deep drawn parts?
It is intended for shallow drawing. Deep drawn components with high draw ratios should be moved to DC04 or DC05, which have lower yield strength and higher elongation.
Q: Does surface grade affect stamping performance?
Yes. Surface grade FB or FC material has fewer defects, so it resists cracking and scoring better than a standard surface finish when visible external panels are produced.