Key Takeaways
SPCC is the JIS G3141 general-purpose cold rolled steel; JSC270C is a deep-drawing grade from the JFS A 2001 automotive series with better formability.
Both are low-carbon cold rolled products, but they target different forming demands: SPCC for simple bending, JSC270C for drawn and automotive panels.
Cross-standard guidance: SPCC roughly corresponds to EN 10130 DC01 (legacy DIN ST12); JSC270C sits in the deep-drawing range, closer to DC03/DC04 territory.
Mechanical values and surface finish must be confirmed against the mill COA and the current edition of the applicable standard.
Two Grade Families, Two Standards
SPCC is a grade from JIS G3141 (cold-reduced carbon steel sheet and strip), the general-purpose grade of that family, followed by SPCD (deep drawing) and SPCE (extra deep drawing). Surface finish and edge condition are designated separately, for example SPCC-1B denotes a bright-finish surface. JSC270C comes from the JFS A 2001 series used by Japanese automotive steelmakers, where JSC270A is the general grade and JSC270C the deep-drawing grade (JSC270D/E for extra deep drawing). The "270" refers to the tensile-strength class and the letter to the forming category.
SPCC vs JSC270C: The Practical Differences
| Aspect | SPCC (JIS G3141) | JSC270C (JFS A 2001) |
|---|---|---|
| Category | General purpose | Deep drawing |
| Typical use | Bending, light forming, panels, general sheet metal | Drawn automotive and appliance parts, complex panels |
| Formability | Standard, adequate for simple operations | Improved drawability with controlled chemistry and annealing |
| Typical mechanicals | Per JIS G3141 tables | Per JFS A 2001 tables |
Exact yield, tensile and elongation values are grade- and thickness-dependent; use the values in the current standard edition or the mill COA, not generic figures.
Cross-Standard Equivalence Guidance
European buyers often ask how these grades map to EN 10130 and to the legacy German designations. The former DIN 1623 designations ST12, ST13 and ST14 were superseded by the EN 10130 DC family - ST12 by DC01, ST13 by DC03 and ST14 by DC04. In that framework, SPCC is broadly comparable to DC01, while JSC270C, as a deep-drawing grade, falls closer to the DC03/DC04 range. Equivalence tables differ between mills; treat them as guidance and confirm the target properties in the order.
How to Specify
- Choose the forming category: general (SPCC/DC01), deep drawing (SPCD/JSC270C/DC03) or extra deep drawing (SPCE/JSC270D/DC04 and above).
- State thickness, width, coil or sheet, and surface finish (for example SPCC-1B or JSC270C equivalent).
- Confirm the standard edition and request the mill COA for the supplied lot.
- For automotive part approval, specify the customer drawing requirement (for example JFS A 2001) explicitly.
Packaging and Shipping

Frequently Asked Questions
Q1. Is JSC270C the same as SPCC?
No. SPCC is a general-purpose JIS grade; JSC270C is a deep-drawing grade in the JFS A 2001 automotive series with better drawability.
Q2. What does SPCC-1B mean?
SPCC is the general-purpose cold rolled grade and 1B designates a bright surface finish under JIS G3141.
Q3. What is DC01 equivalent to?
DC01 (EN 10130, material 1.0330) is broadly equivalent to SPCC for general forming, and replaced the legacy DIN ST12 designation. Confirm properties per the current standard.