Q235, Q235B, Q355 and A36 appear together in countless plate enquiries, yet they belong to different standard families with different philosophies. Q235 and Q355 are Chinese designations from GB/T 700 and GB/T 1591, named after their minimum yield strength in MPa, while A36 is an American designation from ASTM A36, named after 36 ksi (about 250 MPa). Selecting the right grade requires comparing guaranteed properties, impact requirements and the applicable standard of the project.
1. Reading the Grade Names
In GB/T 700, Q235 means a minimum yield strength of 235 MPa; the suffix letter indicates impact quality: Q235A has no impact requirement, Q235B guarantees 27 J at 20 °C, Q235C at 0 °C and Q235D at -20 °C. In GB/T 1591, Q355 guarantees a minimum yield of 355 MPa, with grades B, C, D and E guaranteeing 34 J at 20 °C, 0 °C, -20 °C and -40 °C respectively. In ASTM A36, the number 36 refers to 36 ksi (250 MPa) minimum yield, and the standard covers plates, bars and shapes with specified tensile and elongation requirements. Note that Q345, the predecessor of Q355 under older editions of GB/T 1591, was redesignated Q355 in GB/T 1591-2018.
2. Mechanical Properties Compared
| Grade (standard) | Min. yield (t ≤ 16 mm) | Tensile strength | Min. elongation | Impact requirement |
|---|---|---|---|---|
| Q235B (GB/T 700) | 235 MPa | 370-500 MPa | 26% | 27 J at 20 °C |
| A36 (ASTM A36/A36M) | 250 MPa | 400-550 MPa | 20-23% (by gauge length) | Not specified |
| Q355B (GB/T 1591) | 355 MPa | 470-630 MPa | 22% (thickness-dependent) | 34 J at 20 °C |
Q355D and Q355E add guaranteed low-temperature toughness: Q355D is suitable for service down to -20 °C (for example northern regions, Kazakhstan, Canada) and Q355E down to -40 °C (Arctic, high-altitude sites). Where even lower temperatures are expected, special low-temperature steel grades should be discussed with the supplier on a project basis.
3. Typical Application Fields
Q235 and Q235B plates serve general structural purposes: building frames, platforms, fencing, supports, machine bases and mild forming, where 235 MPa yield is sufficient. A36 is the default structural plate for US-specified projects: bridges, buildings, equipment frames and fabricated members designed to ASTM standards. Q355 plates are used where higher strength saves weight: high-rise structures and bridges, crane booms, truck frames, ship hulls, wind turbine towers, pressure-vessel supports and heavy machinery frames. In the energy sector, Q355 is common for power-plant steelwork and oil and gas facilities, especially in cold-region grades.
4. Supply, Packaging and Processing Considerations
For conventional sizes (thickness 3-50 mm, width 1500-2000 mm, length 6000-12000 mm) and common grades (Q355B/C), plates are typically available from stock with short lead times; non-standard sizes and special grades (Q355D/E, thickness above 50 mm) are rolled to order with longer lead times and larger minimum quantities. Processing such as cutting, drilling, bending and welding extends lead time according to complexity. Export packaging normally combines waterproof wrapping, steel-strap bundling and fumigated wooden pallets to protect against moisture during ocean transit; standard and customized packaging options should be agreed in the purchase order.
Frequently Asked Questions
What is the difference between Q235A and Q235B? Only the impact quality: Q235B guarantees 27 J at 20 °C while Q235A has no impact test requirement; chemistry limits are nearly identical, so Q235B is preferred where notch toughness matters.
Can A36 replace Q235B in a Chinese project? Mechanically A36 (250 MPa yield) is slightly stronger than Q235B (235 MPa), but the project standard must be followed; for design equivalence, verify thickness, elongation and welding consumable compatibility.
Which Q355 grade is right for cold regions? Q355D for service down to -20 °C and Q355E down to -40 °C; confirm the lowest expected service temperature of the structure before specifying.
What does the elongation value depend on? On thickness and gauge length; GB/T 700 and GB/T 1591 give stepped requirements that decrease with thickness, and ASTM A36 specifies values for 200 mm and 50 mm gauge lengths.
How are export plates usually packaged? Typically steel-strap bundling on fumigated wooden pallets with waterproof film wrapping, protecting edges and surfaces during ocean shipping; specify packaging in the order.
Is Q355 weldable with standard procedures? Yes, Q355 is designed as a weldable structural steel; use a qualified welding procedure with appropriate consumables, and consider preheat for thick plates or high restraint per the WPS.