Q:What are the common surface quality problems in cold rolling process?
A:Scratches/abrasions: Linear or flaky scratches appear on the surface of the strip, which may penetrate the entire thickness in severe cases.
Roller marks (indentations): Periodic concave and convex marks appear on the surface of the strip, corresponding to the circumference of the roller.
Adhesion (roller adhesion): After rolling, the strip layers adhere to each other and are difficult to separate.

Q:What are the common causes of surface quality problems?
A:Scratches/abrasions: There are protrusions or foreign objects on the surface of the rollers, guide plates, and straightening rollers; Insufficient tension causes the strip to deviate and rub against the equipment; Incomplete pickling causes the residual iron oxide to fall off after rolling.
Roller marks (indentations): Wear, cracks, or metal debris on the surface of the roller; Foreign objects are pressed into the roller surface during rolling (such as iron filings, lubricating impurities).
Adhesion (rolling adhesion): The rolling speed is too high or the reduction rate is too large, resulting in local temperature rise and welding; Insufficient lubrication, metal direct contact and bonding.

Q:What are the solutions to common surface quality problems?
A:Scratches/abrasions: Check the roller surface accuracy regularly, grind or replace the roller in time; adjust the tension control system to ensure stable operation of the strip; optimize the pickling process to ensure surface cleanliness.
Roller mark (indentation): Use wear-resistant materials (such as high-chromium cast iron) to manufacture rollers, and perform regular flaw detection; strengthen the filtration of the lubrication system and use clean rolling oil.
Adhesion (rolling adhesion): Reduce the rolling speed or control the reduction rate in stages; increase the amount of lubricant or replace high-viscosity rolling oil.

Q:What are the causes and solutions for uneven thickness during cold rolling?
A:Causes: Uneven roll wear or inconsistent thermal expansion; Automatic thickness control (AGC) system response lag or sensor error.
Measures: Use thermal roll shape control technology (such as segmented cooling rolls); Upgrade the AGC system and use a high-precision laser thickness gauge for real-time feedback.
Q:What kind of effects can excessive work hardening easily produce?
A:Phenomenon: After cold rolling, the material strength is too high, the plasticity is insufficient, and subsequent processing is prone to cracking.
Cause: The total reduction rate is too large, and intermediate annealing is not carried out in time; Improper annealing process parameters (such as too low temperature, insufficient time).
Solution: Reasonably design the rolling passes and control the reduction rate of each pass; Optimize the annealing system according to the material grade (such as increasing the annealing temperature or extending the insulation time).