1.What are the reasons related to the materials themselves?
Incorrect Material Grade and Temperament Selection:
Using fully hardened material (e.g., SPCC-1B/4B, DC01-H): This is the most common cause. The material was not annealed after cold rolling, resulting in severe work hardening, extremely low plasticity and elongation, and almost incapable of withstanding any significant bending deformation.
Solution: Select annealed material (e.g., SPCC-1A/4A, DC01-S) or semi-hardened material based on the bending angle and radius.
Substandard or Uneven Mechanical Properties:
Insufficient Elongation: The material's elongation is too low to meet bending process requirements.
Excessive Strength (Yield Strength YS, Tensile Strength TS exceeding standards): Usually accompanied by a decrease in elongation.
Performance Fluctuations: Large performance differences between the same coil of steel or different batches lead to instability in the process window.
Solution: Verify the material quality certificate to ensure that yield strength, tensile strength, and elongation meet standards; conduct incoming material performance sampling inspections for critical components.

2.What are the causes of surface and internal defects?
Edge defects: Burrs, cracks, flash, etc., become stress concentration points during bending, directly inducing cracking.
Internal inclusions (oxides, sulfides): During deformation, inclusions separate from the matrix, forming micropores, which, upon connection, lead to cracking.
Solutions: Inspect the edge quality of the sheet metal; require the supplier to control the purity of the steel produced.

3.What are the consequences of bending in the wrong direction?
Bending parallel to the rolling direction: This is a critical taboo. Cold-rolled coils exhibit significant anisotropy; the plasticity in the transverse direction (perpendicular to the rolling direction) is generally far greater than in the longitudinal direction. The bend line must be perpendicular to the rolling direction.
Solution: Clearly identify the rolling direction during layout and blanking, and strictly adhere to the principle that the bend line must be perpendicular to the rolling direction.

4.What are the consequences of unreasonable bending process parameters?
Insufficient bending radius (R angle): This is the most direct cause of the problem due to manufacturing processes. The tensile strain of the outer fiber layer is directly proportional to tR (material thickness/bending radius). If R is too small, the outer layer strain will exceed the material's limit, leading to cracking.
Solution: Strictly adhere to the recommended minimum bending radius for the material (typically 0.5t-2t, where t is the thickness, depending on the material and its condition). Thicker or harder materials require a larger R angle.
5.What other relevant factors are there?
Improper placement of cuts and holes: Punching, chamfering, or cutting near the bending area severely weakens the cross-section and creates stress concentration, leading to cracking at these locations.
Low ambient temperature: At low temperatures, the toughness of steel decreases (cold brittleness), making it more prone to cracking.
Improper material storage: As discussed earlier, prolonged exposure to sunlight can lead to material property degradation or changes in surface condition, indirectly affecting bending performance.