What causes the markings on cold-rolled coils?

Feb 25, 2026 Leave a message

1.What are the essence and characteristics of roller printing?

Morphology: These are mostly dot-like, short line-like, or long strip-shaped pits or bumps, distributed periodically or continuously on the strip surface.

Tactile Feel: Slight roller marks are not noticeable to the touch, while severe ones are clearly tactile.

Routine: The spacing of the defects usually corresponds to the circumference of the roller that caused the problem; this is a key clue for tracing the source of the defects.

Visual Signs: Some are visible to the naked eye, while others require polishing with an oilstone to be detected.

cold-rolled coil

2.What are the specific causes of defects in the rolling mill rolls themselves?

The rolls may have scratches or grinding marks left during grinding; or the roll surface may have localized chipping or peeling due to fatigue or insufficient hardness; or the roll surface may have scratches or bright spots.

The defects are directly "copied" onto the strip steel, with the cycle being consistent with the circumference of the rolls.

cold-rolled coil

3.What are the specific causes of foreign object indentation/adhesion?

Foreign matter (such as iron filings, dust, sludge, and scale) enters the rolling mill or roll system and is pressed into or adheres to the roll surface. This also includes metal filings detached from edge defects in the raw material (such as burrs and cracks).

The most common cause is foreign objects causing localized bulges on the roll surface, pressing indentations (or protrusions) into the strip.

cold-rolled coil

4.What are the specific causes of process and roller system abnormalities?

Tension rollers and furnace rollers, due to long-term use, suffer from surface coating wear and adhesion nodules (such as eutectic products formed by Mn and Si elements in high-strength steel on the furnace roller); roller body tilting or non-level installation leads to local stress concentration, which, combined with tiny high points on the roller surface, produces roller marks.

Defects may occur in non-rolling processes (such as annealing and rewinding), and their causes are more subtle.

 

5.How to troubleshoot and resolve this issue?

**Measure the cycle, find the source:** Measure the distance between two adjacent roll marks on the strip. This distance is usually the circumference of the roll causing the problem. Based on the circumference, identify the type of roll (e.g., work roll, tension roll, furnace roll).

**Inspect the roll surface, remove foreign objects:** After identifying the suspected roll system, stop the machine and inspect the roll surface for any adhered foreign objects, nodules, peeling, or wear. If it's foreign matter, clean it; if the roll itself is damaged, it needs to be ground.

**Control the source, prevent recurrence:**

**Improve cleanliness:** Regularly clean the machine frame of sludge, control the iron powder content in the emulsion, and implement closed management of clean areas to reduce dust sources.

**Control raw materials:** Inspect the edge quality and internal inclusions of hot-rolled incoming materials to reduce foreign object sources.

**Standardize roll grinding:** Establish a strict roll grinding and pre-machine inspection system to prevent defective rolls from being used.

Optimize the process: for example, adjust the service life of the tension roller and optimize the atmosphere of the annealing furnace to prevent nodule formation on the furnace roller.