1.What are the main effects of white rust on weldability?
Mechanism: White rust is porous and absorbs and stores moisture from the air. Under the instantaneous high temperature of the welding arc, this moisture evaporates rapidly into water vapor. Simultaneously, the white rust itself (ZnCO₃·Zn(OH)₂) decomposes to produce CO₂ and H₂O.
Consequences: These gases, unable to escape before the molten pool rapidly cools and solidifies, become trapped within the weld metal, forming dense porosity. Porosity severely reduces the effective cross-sectional area of the weld, leading to a sharp decline in strength, toughness, and fatigue life.

2.What are the effects of a thick and dense oxide layer or red rust on weldability?
Extremely severe porosity and slag inclusions: The thick oxide layer introduces massive amounts of gas and impurities, making it virtually impossible to achieve a dense weld. The weld will be filled with pores and slag inclusions.
Extremely poor weld quality: Such welds have almost no mechanical properties and represent a serious structural defect, requiring complete removal and re-welding.
Exhausted zinc plating: At this point, the effective zinc coating on the surface has been destroyed, and the welded area has lost the corrosion protection benefits of zinc plating.

3.What are the negative effects of substrate rust (red rust) on weldability?
Iron oxides are non-conductive, difficult to melt, and produce gas. Severe slag inclusions and porosity prevent weld formation.

4.What are the steps involved in mechanical cleaning?
Tools: Angle grinder
Accessories:
Bowl-shaped wire brush: Suitable for cleaning flat surfaces and welds.
Abrasive wheel/louvered blades: For thicker oxide layers or red rust, a more abrasive blade is required.
Standard: Grind until the surface has a uniform metallic sheen, without any white or red spots.
5.How to clean it?
Blow away all dust with compressed air.
If necessary, wipe with acetone or a specialized cleaner to remove any remaining oil or grease.