DC01 Carbon Steel Coil: Properties, DC01 vs DC04 Differences and Plate Sizing Guidance

Aug 26, 2025 Leave a message

DC01 is one of the most widely specified cold rolled carbon steel grades in international trade. It belongs to the DC family of flat products for cold forming defined in EN 10130, and it is the grade buyers encounter first when a component needs clean bending, flanging, coining or shallow drawing at a competitive material cost. This article reviews the grade data behind DC01, explains where it stops and DC04 begins, and gives practical guidance for ordering cut-to-size plates such as 4 mm x 1400 mm x 760 mm.

What Does the DC01 Designation Mean

Under EN 10130, the designation is read in three parts. The letter D indicates a flat steel product intended for cold forming. The letter C states that the product is cold rolled. The two-digit number is a serial number that ranks the grade by forming capability: 01 is the general forming level, 03 the drawing level, 04 the deep drawing level, and 05 and 06 the extra and super deep drawing levels. DC01 is therefore the entry grade of the family, supplied as cold rolled strip, sheet and coil with a smooth, tight surface suitable for painting or for subsequent metallic coating.

Chemical Composition of DC01 (EN 10130)

DC01 is a low carbon, unalloyed steel. The guaranteed maximum values in EN 10130 keep the material soft and stable during cold work:

Element Maximum content (%)
Carbon (C) 0.12
Manganese (Mn) 0.60
Phosphorus (P) 0.045
Sulphur (S) 0.045

The low carbon ceiling is what gives DC01 its characteristic softness: it bends without edge cracking, holds a clean flange, and welds readily with conventional processes.

Mechanical Properties of DC01

For the common thickness range of 0.7 mm to 3.0 mm, EN 10130 guarantees the following values:

Property DC01 value
Yield strength Re (MPa) 140 - 280
Tensile strength Rm (MPa) 270 - 410
Elongation A80 (min %) 28

Note that DC01 does not carry guaranteed r90 (plastic strain ratio) or n90 (strain hardening exponent) values. That is precisely the difference from the drawing grades: DC03, DC04 and higher are tested for these deep drawing indicators, DC01 is not.

DC01 vs DC04: Where Forming Requirements Differ

DC04 is often described as the deep drawing member of the family, and the difference is measurable, not cosmetic:

Property DC01 DC04
Typical use General forming, bending, shallow drawing Deep drawing, complex deformation
Yield strength Re (MPa) 140 - 280 140 - 210
Tensile strength Rm (MPa) 270 - 410 270 - 350
Elongation A80 (min %) 28 38
Carbon (max %) 0.12 0.08

Because DC04 contains less carbon and manganese, it work-hardens more slowly and stretches further before necking. A part with a deep cup, a sharp corner or a severe draw ratio should be quoted in DC04 or above. A simple bent bracket, a flanged plate or a light stamping is normally economic in DC01.

Specifying Cut-to-Size Plate: Notes on 4 mm x 1400 mm x 760 mm

EN 10130 covers cold rolled flat products up to roughly 3 mm nominal thickness. When a requirement arrives as 4 mm x 1400 mm x 760 mm, two supply routes exist. The first is a cold rolled plate produced outside the standard thickness envelope under a bilateral tolerance agreement, which is uncommon. The second, and more usual, route is a hot rolled plate: hot rolled equivalents such as DD11 under EN 10111 or SPHC under JIS G 3131 are the natural choice at 4 mm, with the DC01-type softness approximated by the low carbon DD11 chemistry. Before ordering, the buyer should confirm which route the supplier quotes, because the dimensional tolerances, surface class and mill test certificate will follow the actual standard applied, not the name on the drawing.

Frequently Asked Questions

Is DC01 the same as CR4 or St12?

Roughly, yes. CR4 is the traditional British designation for this soft cold reduced steel, while St12 is the former DIN designation that EN 10130 replaced with DC01. The steel number 1.0330 is common to all three naming systems.

Can DC01 be welded?

Yes. Its low carbon content makes it suitable for MIG, TIG, resistance spot welding and most conventional arc processes without preheat. The surface oil film should be removed at the joint area, and for galvanized or painted DC01 the coating must be dressed back before welding to avoid fume and porosity.

Does DC01 need surface protection in storage?

As delivered it usually carries a light protective oil film. In humid or coastal warehouses the coil should stay wrapped, and cut plate edges should be oiled or primed, because the bare low carbon surface rusts quickly once condensation forms.

What surface quality can be expected?

EN 10130 defines surface classes A, B and C. Class A suits visible, high-gloss painted panels; class B is the common general purpose level; class C allows visible imperfections and is used where surface finish is not critical. The class should be written into the order.

Is DC01 suitable for galvanizing?

Yes, and it is the dominant substrate for continuously hot-dip galvanized and galvannealed strip. The clean cold rolled surface reacts well with the zinc bath, which is why DX51D under EN 10346 is essentially a DC01-type base with a metallic coating.

Why is a 4 mm DC01 plate unusual?

Cold rolling above about 3 mm becomes uneconomic and is outside the EN 10130 scope, so 4 mm requirements are normally met with hot rolled low carbon material. Always confirm the governing standard before accepting a quotation for a 4 mm cold rolled plate.