DC01, DC06, St37-2 and Galvanized Coil: Matching Grade to Product

Sep 29, 2025 Leave a message

Four Product Families Behind One Search Term

Enquiries that combine designations such as DC01, DC06, St37 and galvanised coil are usually trying to describe several different products with one phrase, and clarifying which family is actually required is the fastest way to avoid a wrong delivery. Cold-rolled drawing grades DC01 to DC06 are defined in EN 10130 and are supplied uncoated. Structural hot-rolled grades such as St37-2 belong to the former DIN 17100 system and are now covered by EN 10025-2. Continuously hot-dip coated coil is described by EN 10346, and electrolytically zinc coated coil by EN 10152. The four families are produced on different lines, tested against different property tables and priced on different bases, so a single order line cannot cover them all.

The confusion is understandable because the codes overlap in conversation. A fabricator may hold DC01 sheet in stock, order St37 angle for a frame, and buy galvanised coil for cladding, and all three may appear on the same requisition as mild steel. The mistake to avoid is treating one as a substitute for another: a drawing grade is specified on formability, a structural grade on yield strength and impact behaviour, and a coated grade on coating mass and corrosion life.

St37-2 and Its Modern Equivalent

Property S235JR per EN 10025-2
Minimum yield strength ReH, thickness up to 16 mm 235 MPa
Tensile strength Rm 360-510 MPa
Minimum elongation A 26 %
Maximum carbon 0.17 %
Maximum manganese 1.40 %
Maximum phosphorus and sulphur 0.045 % each

St37-2 was the designation used in DIN 17100 for a general structural steel with a minimum yield strength of 235 MPa, and that standard has been withdrawn in favour of EN 10025-2, where the corresponding grade is S235JR. In the new code S marks structural steel, 235 is the minimum yield strength in megapascals, J denotes a minimum impact energy of 27 joules and R indicates that the impact test is performed at room temperature. Older drawings that still show St37 or St37-2 should be translated into the EN designation on the purchase order, together with the deoxidation and impact requirements, because the two systems are compatible in strength but not identical in every delivery condition.

Because these are hot-rolled products, thickness tolerances, surface condition and edge condition differ from cold-rolled sheet, and the material normally arrives with mill scale unless it is supplied pickled. Where a structural part will be painted, the scale and the surface preparation route affect the coating system, and where it will be galvanised, the galvaniser's process is designed around the mill scale and the steel chemistry.

Cold Rolled Drawing Grades DC01 and DC06

DC01 and DC06 sit at opposite ends of the EN 10130 family. DC01 is the entry grade, with carbon capped at 0.12 %, a tensile range of 270-410 MPa and an elongation floor of 28 % over an 80 mm gauge length, and it is used for bending, beading and shallow forming. DC06 is a stabilised, interstitial-free grade produced for the most severe drawing operations: titanium or niobium additions remove the interstitial carbon and nitrogen from solution, which eliminates ageing and delivers the highest elongation and plastic strain ratio values in the family. Mechanical testing of both grades follows ISO 6892-1, with the formability ratios measured in accordance with ISO 10113 and ISO 10275 where they are specified.

The practical choice between them is a matter of draw severity and of ageing behaviour. DC01 can sit in stock for months and still form predictably because its properties do not depend on a stabilising addition, while an unstabilised deep drawing grade that has been stored for a long period can lose ductility through strain ageing. DC06 avoids that problem entirely and is consequently the grade of choice for critical panels that are formed after long storage or transported between sites before pressing.

Galvanised Coil: Substrate and Coating Data

Item Typical galvanised coil per EN 10346
Grade designation DX51D+Z, DX53D+Z, DX54D+Z
Coating type Z pure zinc, ZF zinc-iron alloy, ZA, AZ, ZM alloys
Coating mass, total both surfaces Z100 to Z450 g/m²
Coating thickness, Z100 about 7 µm per face
Coating thickness, Z275 about 19 µm per face
Tensile strength, DX51D+Z 270-500 MPa

Coating mass is quoted as the total zinc on both surfaces, and the conversion to coating thickness uses the density of zinc at 7.14 g/cm³: divide the single-face mass by 7.14 to obtain micrometres. Corrosion life in a given atmosphere follows the coating mass far more closely than it follows the substrate grade, which is why a Z275 coil outlasts a Z100 coil of the same steel by a factor of roughly two to three. Coating type changes the surface as well: a zinc-iron alloy surface is harder, more abrasion resistant and better suited to painting, while a pure zinc surface is more ductile in bending. Dimensional tolerances for these coated products are given in EN 10143.

It is worth distinguishing continuously coated coil from batch galvanising of fabricated articles. Coil is coated in a continuous line to a declared coating mass, while finished structures, sections and fabrications are hot-dip galvanised to EN ISO 1461, which sets a minimum local coating thickness by article thickness: 70 µm for material between 3 mm and 6 mm, and 85 µm for material above 6 mm. The two routes produce different coating structures and are specified by different standards, so a requirement written for one cannot be applied to the other.

Matching Grade to Application

Roof and wall cladding, ducting and general panelling normally use DX51D+Z or a comparable commercial-quality coated grade, with the coating mass chosen for the exposure and the expected service life. Pressed panels and formed housings that need both corrosion protection and drawing quality use DX53D+Z or DX54D+Z. Structural frames, brackets and supports use S235JR hot-rolled product, either painted or, after fabrication, batch galvanised to EN ISO 1461. Parts that are formed before being assembled into a structure usually work better as coated coil, because the coating is applied before forming and the press tooling is designed around the coated surface.

Two purchasing points reduce risk across all four families. First, state the standard, the full grade designation including coating type and mass where relevant, and the tolerance class, since the grade code alone leaves too many open variables. Second, state the inspection document level under EN 10204, because a 3.1 certificate gives measured values for the delivered heat and allows an incoming inspection to confirm the material in a few minutes rather than after a failed forming run.

Frequently Asked Questions

Q: Can St37 be ordered as S235JR?
A: Yes. DIN 17100 St37-2 was replaced by EN 10025-2 S235JR, where 235 is the minimum yield strength in megapascals, J is a minimum impact energy of 27 joules and R means the impact test is carried out at room temperature.

Q: Is continuously galvanised coil the same as hot-dip galvanised steelwork?
A: No. Coil is coated on a continuous line to a declared coating mass under EN 10346, while fabricated articles are batch galvanised under EN ISO 1461, which requires a minimum local thickness of 70 µm for material 3 mm to 6 mm thick.

Q: Which grade should be used for roof and wall panels?
A: A commercial-quality coated grade such as DX51D+Z, with the coating mass selected for the exposure. Forming severity, not the panel name, decides whether a drawing grade such as DX53D+Z or DX54D+Z is required.

Q: What is the difference between DC01 and DC06?
A: DC01 is the entry drawing grade with a 28 % elongation floor and no guaranteed formability ratio. DC06 is a stabilised, interstitial-free grade with the highest elongation and plastic strain ratio in the family and no ageing risk during storage.

Q: Can S235JR be galvanised after fabrication?
A: Yes, by batch hot-dip galvanising to EN ISO 1461. The steel chemistry and the surface condition influence coating quality, and the design of the fabrication has to allow drainage and venting for a uniform coating.

Q: How is coating mass converted into coating thickness?
A: Zinc has a density of 7.14 g/cm³. Divide the coating mass on one surface by 7.14 to obtain thickness in micrometres, so Z100 corresponds to 50 g/m² per face and therefore about 7 µm per face.