DC05 Deep Drawing Steel: r-Value, n-Value and Press Settings That Work

Oct 12, 2026 Leave a message

DC05 is the extra-deep-drawing grade of EN 10130: yield strength 180 MPa maximum, tensile strength 270-330 MPa, elongation A80 of at least 40%, r90 at least 1.9 and n90 at least 0.20. Those last two numbers are the reason the grade is specified at all, so this page explains what they do on the press, how the guarantees move with thickness, and where DC05 stops being the right answer.

DC05 Deep Drawing Steel

 

1.What the Two Extra Numbers Do

 

r90 is the plastic strain ratio. It says whether the steel thins through its thickness or flows in the plane of the sheet. A high r-value thickens the flange instead of thinning the wall, so a deep cup survives the draw. DC05 at r90 ≥ 1.9 holds wall thickness where a lower-r grade starts to neck.

The catch is planar anisotropy, written Δr. A high average r helps the draw, but a wide spread of r with direction grows ears on the rim of the cup. Earing is trimmed off, so it costs material. If rim trim is running high, ask for r in three directions rather than the transverse value alone.

 

n90 is the strain-hardening exponent. High n spreads strain instead of letting it pile into one spot, which delays necking where the part is stretched rather than drawn. DC05 at n90 ≥ 0.20 survives the local stretching that splits DC04 in a panel corner or a tight radius.

 

2.The Guarantees Move with Thickness

 

The headline values hold in the middle of the thickness range. Outside it, EN 10130 adjusts them:

Thickness

Yield strength max

A80 min

r90 min

≤ 0.50 mm

220 MPa

36%

not specified

0.50-0.70 mm

200 MPa

38%

1.9

0.70-2.00 mm

180 MPa

40%

1.9

> 2.00 mm

180 MPa

40%

1.7

Below 0.50 mm, r and n are not defined at all. Above 2 mm, r90 drops by 0.2. For design work the standard allows a lower yield strength of at least 140 MPa to be assumed.

 

Read every certificate against the gauge you bought, not against the grade name. A 0.45 mm strip legitimately reports a higher yield strength and lower elongation than 1.00 mm material of the same grade. That is the standard, not a soft coil.

 

3.Starting Settings on the Press

Every die is different, so take these as a first setup and tune on the trial:

 

Die entry radius around 8-10 × thickness

Punch nose radius around 5-8 × thickness

Clearance 10-15% over thickness, per side

Blank-holder pressure starting at 1.5-3 MPa on the flange, raised only as far as wrinkles demand

Lubricant an EP drawing compound, washed off before welding, painting or plating

Speed moderate. Very fast draws give the material less time to flow

 

As an indicative measure of how far the grade will go, DC05 typically reaches a limiting drawing ratio of about 2.1-2.2 under standard tooling, against roughly 2.0 for DC04. That is a comparison between grades, not a promise for your part; tooling, lubrication and blank-holder control decide the real figure. Cupping tests on DC05 normally return 9 mm and above at around 1 mm thickness.

 

4.Where DC05 Is Not the Answer

Shallow parts. If the draw is easy, DC04 does the work for less money.

The hardest draws. Fuel tanks and very deep shells usually move to DC06, which is stabilised and carries no time limit on freedom from stretcher-strain marks.

Strength-led designs. DC05 is soft by design. Where the part needs strength after forming, a higher-strength grade buys it and gives up formability.

Long outdoor storage. Cold rolled steel has no corrosion resistance of its own; the oil protects it for months, not indefinitely.

 

5.Packaging and Shipping

Packaging and Shipping
Packaging and Shipping
Packaging and Shipping
 
 
 

6.FAQ

Why is yield strength given as a maximum?

Because drawability comes from being soft. A lower number is better, not weaker than spec.

Do r90 and n90 appear on every certificate?

Only where they are asked for at enquiry and order. Say so in writing.

Will DC05 stop springback?

Its low yield strength reduces the elastic energy behind springback, which helps, but geometry and blank-holder control still decide the final shape.

Can we trial before committing?

Yes. Ask for a sample coil from the same heat so the trial reflects production rather than a random piece of stock.

 

Talk to Us About the Draw

Send the part drawing, or the draw depth and corner radii, plus the thickness you need and the press you run. We will tell you whether DC05 is the right grade or whether DC04 or DC06 fits better, and quote coil or slit strip within 24 hours.

 