Raw Material Defects
Inappropriate coil diameter: thin hot-rolled coils can shrink and droop at the inner ring during cooling, reducing the inner diameter; remove the inner ring by gas cutting. Uneven and cracked edges: caused by equipment and side guides during coiling and improper lifting tools during transport; adjust equipment and change lifting tools. Sickle bend: caused by wedge-shaped slabs or unequal roll gaps producing uneven deformation; stabilize the roller side guides and adjust tension. Tail edge wave: caused by excessive rolling force, uneven roll wear, or coiler segment wear; replace worn blocks and control rolling parameters. Width variation: super wide ends and narrow middle from tension variations; set suitable tension values.
Pickling Defects
Under-pickling: unwashed iron oxide remains on the surface, appearing dark or stained after rolling. Causes include short pickling time, low acid concentration, insufficient acid, and poor turbulence. Treatment: ensure concentration, temperature, and spray are in range, enhance acid flow, and control process speed. Over-pickling: the strip stays too long in the acid and the substrate is corroded, producing a rough, pitted surface and reduced ductility. Treatment: reduce acid concentration and temperature, reduce spray volume, and add corrosion inhibitors that form a protective film. Water rust: residual acid not rinsed or poor drying causes rust at edges; check squeeze rollers, spray pressure, dryer temperature, and rinse water conductivity. Parking spot: when the line stops, the strip section in acid and water is over-pickled and rusted; ensure equipment reliability to avoid stops.
Surface Defects
Heavy skin: local stratification on the strip surface, mostly at the head or edge, connected along the rolling direction, often appearing after cold rolling and severe cases causing holes and broken strips. Scarring: surface heavy areas of different shapes with inclusions or iron oxide scale. Scratches: regular scratches are located by their spacing to identify the source section; irregular scratches come from uneven strip running, unstable tension, or poor plate shape; keep equipment running normally and improve plate shape.
Edge and Appearance Defects
Edge defects from the trimming shear include uneven shearing, gaps, uncut waste edges, and burrs, caused by wrong knife gap settings, heavy knife weight, broken knives, or excessive knife wear; inspect and adjust knife settings and replace worn knives. Tower defects at the coiler, where the tower exceeds 30 mm on one side, are treated as scrap; level the belt winder, adjust the belt threading program to wind more turns before opening the belt assistant, and widen the belt.
Quality Improvement Approach
Strengthen quality management with detailed rules implemented layer by layer; improve employee skills through continuous training from theory to practice; and build technical cooperation with users for material selection, usage problem solving, and full-process technical solutions.
Frequently Asked Questions
Q: What causes under-pickling?
Short pickling time, low acid concentration, insufficient acid, and poor turbulence leave iron oxide on the surface.
Q: How is over-pickling prevented?
Reduce acid concentration and temperature, control spray, and add corrosion inhibitors to protect the substrate.
Q: What is water rust?
Rust formed at edges when residual acid is not rinsed or drying is poor after pickling.
Q: What causes sickle bend?
Wedge-shaped slabs, uneven slab thickness, or unequal roll gaps producing uneven deformation.
Q: How are regular scratches located?
By measuring the spacing between scratches to identify which line section produces them.
Q: When is a tower defect scrapped?
When the tower on one side of the coil exceeds 30 mm.