What DC04 Means in EN 10130
DC04 is a cold-reduced, low-carbon flat steel product for cold forming, defined in EN 10130 together with DC01, DC03, DC05 and DC06. The letters stand for drawing quality, and the trailing digits rise with formability: DC01 is general drawing quality, DC03 is deep-drawing quality and DC04 is special deep-drawing quality intended for parts with severe deformation, tight radii and pronounced wall thinning. Because EN 10130 controls both chemistry and the forming parameters, a DC04 coil is defined less by its strength than by its ability to be pressed into shape without necking or tearing.
That is why DC04 is normally quoted with a maximum yield strength rather than a minimum. Too much yield strength is a drawback in deep drawing, since it makes the material spring back and resist flow into the die. The standard therefore caps the upper yield limit, sets a minimum elongation, and specifies a minimum plastic strain ratio so that the sheet thins evenly instead of localising strain in one band.
DC01, DC03 and DC04 Compared
| Grade | Drawing quality | Typical application |
|---|---|---|
| DC01 | General drawing quality | Simple bends, panels without severe drawing, general fabrication |
| DC03 | Deep-drawing quality | Appliance shells, sinks, housings with moderate draw depth |
| DC04 | Special deep-drawing quality | Complex automotive and appliance parts, severe drawing and profiling |
| DC05 / DC06 | Extra deep-drawing quality | Very severe forming where even DC04 reaches its limit |
Two of these grades are frequently confused with commercial zinc-coated designations. DC01 is also the base metal behind DX51D-class galvanized coil, and DC03 supplies the substrate for higher-ductility coated products. The DC family itself, however, is supplied uncoated unless a coating suffix such as Z or ZE is added, so DC04 ordered plain arrives with a mill surface that must be protected against humidity during transport and storage.
Mechanical and Dimensional Data
| Property | DC01 | DC03 | DC04 |
|---|---|---|---|
| Upper yield strength, max | About 280 MPa | About 240 MPa | About 210 MPa |
| Tensile strength, typical | 270 to 410 MPa | 270 to 370 MPa | 270 to 350 MPa |
| Minimum elongation | About 28% | About 34% | About 38% |
| Forming intent | Bending and lock forming | Deep drawing | Severe deep drawing |
Dimensional practice follows the cold-rolling mill rather than the grade. Standard supply runs from about 0.3 mm to 2.0 mm in thickness, with widths from 600 mm up to roughly 1500 mm as rolled. Coils are normally supplied on a 508 mm or 610 mm inner diameter with an outer diameter up to around 1300 mm, and unit weights up to about 10 t. Sheets are cut to ordered lengths, typically up to 3000 mm, and slit strip is available for progressive-die work where the blank width is fixed by the tooling.
Delivery Forms: Coil, Sheet and Slit Strip
The same DC04 heat can be delivered in three shapes, and the choice affects both handling and yield. Full coils suit high-volume roll forming and press lines with coil feeding equipment. Cut sheets suit job-shop fabrication, laser and shearing operations where the blank size is already known, and manual feeding of older presses. Slit strip suits dedicated lines that run one width continuously and want to avoid scrap at the edges of a wide coil.
Whichever form is ordered, three process variables should be agreed at the enquiry stage: the surface quality class, the surface finish, and the oiling condition. Cold-rolled sheet for exposed parts needs a surface free of roll marks, scratches and emulsion residues, while sheet destined for immediate painting may be supplied lightly oiled to prevent corrosion in transit but not so heavily that degreasing becomes difficult.
Cut-to-length lines introduce their own risks. Levelling that is too aggressive leaves residual stresses and causes parts to twist after blanking, while inadequate levelling leaves coil set and crossbow. For DC04, which is intended for severe forming, the flatness and residual stress condition of the delivered sheet has a direct effect on the failure rate in the press, so flatness tolerances should be written into the order rather than assumed.
Surface Finish, Annealing and Storage
DC04 is produced by cold reduction followed by annealing and a light skin pass. Annealing develops the recrystallised microstructure that gives the grade its ductility, and skin passing controls yield-point elongation and surface texture. Fully finished material is normally supplied skin-passed because unskimmed sheet tends to develop stretcher strain marks at the first forming operation.
Protection after delivery matters as much as the mill process. Plain cold-rolled sheet is unprotected steel; condensation between stacked sheets or under coil wraps produces staining within days in humid conditions. Sheets should be stored flat on dunnage in a dry, ventilated area, and coils should stay wrapped and off the floor. When parts must wait between forming and finishing, or when the service environment is humid, an electro-zinc coated or hot-dip coated variant of the same base grade is the practical alternative.
Frequently Asked Questions
Q: What is DC04 steel?
DC04 is a special deep-drawing quality, low-carbon cold-reduced flat steel grade defined in EN 10130, used where forming severity is too high for DC01 or DC03.
Q: What is the difference between DC01 and DC04?
Both are EN 10130 cold-forming grades, but DC04 has a lower maximum yield strength, higher minimum elongation and better drawability, so it can be pressed into more complex shapes.
Q: Is DC04 the same as SPCC?
No. SPCC is a Japanese commercial cold-reduced grade with no guaranteed drawing performance, while DC04 is a European special deep-drawing grade with specified forming properties.
Q: Can DC04 be supplied with a coating?
Yes. The same base grade is available electro-zinc coated or hot-dip coated when corrosion protection is required, in which case the coating type and mass must be specified.
Q: What thickness range is typical for DC04 coil?
About 0.3 mm to 2.0 mm, with widths from 600 mm to roughly 1500 mm and coil weights up to about 10 t.
Q: Why does the yield strength limit matter for deep drawing?
Because a higher yield strength makes the sheet resist flow into the die and spring back after forming; EN 10130 therefore caps the upper yield value instead of setting only a minimum.