How to test the moisture and heat resistance of galvanized coils?

Oct 16, 2025 Leave a message

1.What are the test standards and test conditions for salt spray test?

Test Standards:

Neutral Salt Spray Test: The most basic method, following ASTM B117 / ISO 9227.

Acetic Acid Salt Spray Test: More severe than neutral salt spray, used to obtain results faster.

Copper-Accelerated Acetic Acid Salt Spray Test: Even more severe, with the shortest cycle time.

Test Conditions:

Solution: 5% sodium chloride solution.

Temperature: Typically maintained at a constant 35°C.

Environment: In a sealed chamber, the salt solution is atomized through a nozzle to create a diffuse salt spray environment.

Humidity: Approximately 100% RH.

Galvanized Coil

2.What are the test standards and test conditions for constant temperature and humidity test?

Test Standard: ASTM D1748 / ISO 6270-2 (commonly known as the "rust preventative oil test," but also applicable to zinc coatings)

Test Conditions:

Temperature: Typically set at 40°C ± 2°C or 50°C ± 2°C.

Humidity: Constantly maintained above 95% RH, or even 100% RH.

Test Duration: Depending on the requirements, this can range from tens to hundreds of hours.

Galvanized Coil

3.What are the test standards and test conditions for cyclic corrosion testing?

Test standards: ISO 14993 / CCT-I, or the proprietary standards of major automakers (e.g., GMW 14872, VW 50185).

Test cycle example (a typical 24-hour cycle):

Salt spray phase: Apply salt spray at 35°C for a period of time (e.g., 1 hour).

Drying phase: Raise the temperature to 60°C and reduce the humidity (e.g., 30% RH) to dry the sample surface.

Wet heat phase: Maintain a high humidity environment at 50°C and 95% RH.

Repeat this cycle.

Galvanized Coil

4.What are the testing process and evaluation metrics?

Sample Preparation:

Cut a specimen of the specified size (e.g., 150mm x 100mm) from the galvanized coil.

Seal the edges of the specimen with tape or wax to prevent corrosion from the cut edge, which could interfere with the assessment of the primary surface.

Clean the specimen surface to remove any oil or fingerprints.

Placement:

Place the specimen at a certain angle (e.g., 15°-30°) on the support inside the test chamber.

Test Duration:

The total test duration is determined based on product specifications or agreement with the customer (e.g., 24 hours, 48 ​​hours, 72 hours, 96 hours, 200 hours, 500 hours, etc.).

Results Evaluation and Recording:

Macroscopic Observation: Regularly observe and photograph surface changes, focusing on the appearance and development of white and red rust.

Quantitative Rating:

Corroded Area Percentage: Evaluates the area covered by rust.

Adhesion Loss: After testing, the zinc layer can be inspected for flaking using the tape method.

Weight Change: For scientific research or precise comparison, the surface is accurately weighed before and after testing to calculate the weight loss (zinc loss) or weight gain (corrosion product formation) per unit area.

 

5.How to interpret the test results?

Time to white rust: This indicates the corrosion rate of the zinc coating itself. A longer time indicates a more stable zinc coating and better resistance to moisture and heat. This is closely related to the zinc coating's purity, thickness, and whether it has been passivated.

Unpassivated galvanized coils have the shortest time to white rust.

Oil-coating or chromium-free passivation can significantly extend the time to white rust.

Chromate passivation (color coating/yellow coating) is most effective because it forms a dense protective film.

Time to red rust: This indicates the protective lifespan of the zinc coating on the steel substrate. This is the final and most important indicator, reflecting the zinc coating's thickness, uniformity, and corrosion rate. The later red rust appears, the longer the product's overall service life.