1.What are the performance indicators of substrates?
Substrate Thickness: The thickness of the cold-rolled steel coil itself determines the sheet's rigidity and resistance to wind and snow loads. The thicker the steel, the greater its load-bearing and deformation resistance.
Zinc Layer Weight: The weight per unit area of the galvanized layer on the substrate surface. This determines the corrosion resistance of the underlying substrate. The thicker the zinc layer, the better it isolates the steel from external corrosive media.
Substrate Yield Strength: The maximum stress the substrate can withstand before undergoing plastic deformation. This determines the sheet's resistance to bending and stretching, preventing permanent deformation caused by loads during installation or use.
Substrate Elongation: The maximum percentage of elongation before the substrate breaks; this influences the sheet's processing properties (such as bending and rolling). The higher the elongation, the less likely it is to crack during processing.

2.What are the coating performance indicators?
The coating is the "outer coat" of the color-coated galvanized coil, which directly resists the erosion of ultraviolet rays, rain, and chemical media. Its performance is the core guarantee of the plate's weather resistance and corrosion resistance. It is divided into coating structure indicators and coating physical performance indicators.
Coating Structure Indicators
Total coating thickness: The combined thickness of primer + topcoat (sometimes including backcoat), typically measured in μm.
Implications: Insufficient thickness can lead to premature wear and exposure of the coating; excessive thickness can cause decreased adhesion and cracking.
General range: ≥60μm for industrial and construction applications (5-10μm for primer + 20-30μm for topcoat, 5-10μm for backcoat); ≥80μm for highly weather-resistant applications (such as coastal areas).
Coating Physical Performance Indicators
Adhesion: The strength of the bond between the coating and the substrate (or primer and topcoat) is key to preventing coating peeling and blistering.
Test Method: Cross-hatch method (draw a cross or grid, peel with tape, and observe for coating peeling). Grades are 0-5 (Grade 0 is optimal, meaning no peeling).
Requirement: Industrial color-coated coils must meet Grade 0 or 1; otherwise, delamination of the coating may occur during processing or outdoor use.
Hardness: The coating's resistance to scratches and impacts is measured using the "pencil hardness" scale (from 6B to 9H, increasing in hardness).
Requirement: The topcoat's hardness must be ≥ 2H to prevent surface scratches caused by friction during installation or transportation, which could affect aesthetics and corrosion resistance.
Flexibility (bending resistance): The coating's ability to withstand bending without cracking or peeling, directly impacting processing suitability (e.g., bending and roll-forming). Test Method: Bend the sheet material around a cylindrical mandrel of varying diameters (e.g., the "T-bend test," with a bend radius equal to n times the substrate thickness, denoted as Tn) and observe whether the coating cracks.
Requirement: Industrial applications typically require a T2-T4 rating (e.g., T2 indicates no cracking at a bend radius of twice the substrate thickness) to ensure coating integrity after processing.
Impact Resistance: The coating's ability to withstand external impacts (such as hail and falling objects) to prevent damage and exposure to the underlying coating.
Test Method: A hammer of a specified weight is dropped from a specified height onto the coating surface to observe for cracks or exposure.
Requirement: The coating must show no visible cracks or exposure to the underlying coating after impact. A common standard is "no damage after impact with a 500g hammer at a height of 50cm."

3.What is the impact on weather resistance and corrosion resistance performance indicators?
Salt Spray Resistance: Simulates coastal and high-salt spray environments (such as marine atmosphere and chemical industrial zones) to test the synergistic corrosion resistance of the coating and zinc layer.
Test Method: Place the sample in a salt spray chamber containing a 5% sodium chloride solution and continuously spray. Observe the time it takes for red rust (steel corrosion) or white rust (zinc corrosion) to appear.
Requirements:
Ordinary Polyester (PE): ≥500 hours without red rust;
Highly Weatherable Polyester (HDP): ≥1000 hours without red rust;
PVDF: ≥2000 hours without red rust (industrial plants in coastal areas must meet at least HDP grade, with PVDF grade preferred).
Accelerated Aging Resistance: Simulates strong UV rays, high temperature, and high humidity to test the coating's weather resistance (to avoid fading, chalking, and cracking).
Test Method: Continuously irradiate the coating for thousands of hours in a xenon arc aging chamber (simulating sunlight) or a UV aging chamber to test color difference and gloss retention. Requirements:
Gloss retention after aging: Standard PE ≥ 50%, HDP ≥ 70%, PVDF ≥ 80%;
Color difference (ΔE): ≤ 3.0 (fading is not noticeable to the naked eye).
Chemical resistance: For special environments such as chemical plants, this test measures the coating's ability to resist corrosion from acids, alkalis, and solvents.
Common tests include neutral salt spray resistance (already mentioned), acid resistance (immersion in 10% hydrochloric acid solution), and alkali resistance (immersion in 10% sodium hydroxide solution). After immersion, the coating must exhibit no peeling, discoloration, or blistering.

4.What is the impact of processing and appearance performance indicators?
Processing performance: In addition to the "flexibility" and "impact resistance" mentioned above, this also includes:
Flatness: The flatness of the board surface to avoid warping and wavy lines that can make installation and splicing difficult, potentially affecting sealing (e.g., roof leaks).
Edge quality: The edges must be free of burrs and curling to prevent scratches on operators or damage to sealants during installation.
Appearance: This affects the visual quality of the building or equipment. Key indicators include:
Color and gloss: The color must meet design requirements. Gloss (at a 60° angle) can be selected as needed (high gloss ≥ 70%, semi-gloss 30%-70%, matte ≤ 30%). The color difference within the same batch must be ≤ 1.5 (to avoid color unevenness).
Surface defects: There must be no obvious pinholes, impurities, scratches, or missing paint. Industry standards generally require "≤ 1 defect per square meter, and the area of each defect ≤ 0.5 mm²."
5.What is the priority of core indicators in different scenarios?
For coastal industrial plants: Prioritize zinc coating weight (≥180g/m2), coating type (PVDF/HDP), salt spray resistance (≥1000 hours), and aging resistance.
For inland general plants: Prioritize zinc coating weight (≥120g/m2), coating type (standard PE/HDP), adhesion (grade 0-1), and flatness.
For chemical/corrosive plants: Additional emphasis should be placed on chemical resistance, coating thickness (≥80μm), and substrate yield strength (≥345MPa).
For home appliances/indoor equipment: Prioritize appearance (low color difference, matte finish), substrate thickness (0.12-0.5mm), and electroplated zinc coating (≥20g/m2).