Key points of quality control in SECC electrogalvanizing process

Sep 19, 2025 Leave a message

1.How to control the degreasing effect?

Core Indicator: Residual oil on the substrate surface ≤ 5mg/m² (verified by the "water film test": After degreasing, rinse the substrate with water. The water film should remain continuously covered for at least 10 seconds without breaking, and there should be no localized hydrophobic spots).
Key Control Points:
Degreaser Concentration: Maintain the concentration of the alkaline degreaser (NaOH + Na₂CO₃) at 5%-8%. Regularly check by titration. If the concentration is too low, replenish it promptly.
Temperature and Time: Bath temperature 40-60°C (temperature difference ≤ ±3°C), immersion/spraying time 3-5 minutes. Avoid temperatures too low (causing incomplete emulsification of oil contamination) or too high (causing degreaser decomposition).
Cleaning Residue: After degreasing, perform two countercurrent rinses. The pH value of the final rinse should be controlled between 6.5-7.5 (check with pH paper or an online pH meter) to prevent degreaser residue from entering the pickling tank and causing "secondary contamination."

SECC

2.What are the key points of pickling effect and anti-corrosion control?

Core Indicators: Complete removal of oxide scale, a uniform gray-white substrate surface (no localized blackening or mottling), and no excessive corrosion (no pitting or dents).
Key Control Points:
Acid Concentration: 15%-20% for hydrochloric acid pickling (10%-15% for sulfuric acid pickling). Test weekly. Add fresh acid if the concentration falls below the lower limit.
Pickling Time: Adjust according to oxide scale thickness (3-10 minutes). Monitor the pickling time using both timed and visual monitoring. Remove the substrate immediately if an "excessive corrosion tint" (e.g., dark gray) begins to appear on the surface.
Corrosion Inhibitor Addition: Add 0.1%-0.3% of a pickling inhibitor (e.g., hexamine) to the pickling solution to inhibit excessive dissolution of the substrate and reduce the risk of hydrogen embrittlement. (SECC substrates are cold-rolled steel, and hydrogen embrittlement can reduce subsequent stamping performance.)

SECC

3.What are the key points of activation and drying control?

The activation tank acid concentration (1%-3% dilute hydrochloric acid) must be stable, and the activation time must be 10-30 seconds to ensure that no "passivation film" remains on the substrate surface (the surface should be matte and uniformly rough after activation).

The drying temperature should be 80-120°C for 1-2 minutes. The moisture content of the substrate surface at exit should be ≤ 0.1% (checked using a moisture meter) to prevent water from entering the plating tank and causing pH fluctuations in the plating solution.

SECC

4.What are the key points of "cleanliness maintenance" of plating solution?

Filtration and Purification:
Use a 5-10μm bag filter to continuously filter the plating solution (filtration rate ≥ 2 times the total plating solution volume/hour) to remove impurities (such as anode mud and substrate debris) and prevent "granular defects" in the coating.
The plating solution is purified weekly (by adding activated carbon to absorb organic impurities) to prevent impurities from causing the coating to become dark and dull.
Anode Management:
Anodes use pure zinc plates with a purity of ≥ 99.95% to prevent impurities (such as iron and lead) from dissolving and contaminating the plating solution.
The anode to cathode area ratio is controlled at 1.2:1-2:1 to ensure even current distribution and prevent areas of thin coating.

 

5.What are the key points of chromate passivation (or chromium-free passivation) control?

Core Indicators: Passivation film thickness 0.5-1μm, no white rust after ≥50 hours in a neutral salt spray test (NSS) (JIS Z 2371 standard).
Key Control Points:
Passivation Solution Concentration: Hexavalent chromium passivation solution (CrO₃ concentration 20-50g/L) or chromium-free passivation solution (titanate/zirconate concentration 10-30g/L). Check the concentration daily to ensure stability.
Treatment Temperature and Time: Room temperature (20-25°C), immersion time 30-60 seconds. Avoid excessively high temperatures that may cause cracking of the film, or excessively short soaking time that may cause film incompleteness.
Post-Passivation Washing: After passivation, rinse once with deionized water (conductivity ≤ 10μS/cm) to prevent residual passivation solution from causing surface rusting. Dry immediately (100-120°C, 1 minute).