Hot-Dip Galvanized Steel Pipe Production Process Explained

Feb 06, 2024 Leave a message

What Hot-Dip Galvanizing Does

Hot-dip galvanizing protects steel pipe by immersing the cleaned pipe in molten zinc. The molten zinc reacts with the iron surface to form a series of zinc-iron alloy layers, with a pure zinc layer on the outside, so the coating is metallurgically bonded rather than merely painted on. This bond gives the coating its toughness: it withstands handling, bending and temperature changes, and it protects the steel both as a barrier and sacrificially at scratches and cut edges. The main advantages of the process are its relatively low processing cost for large quantities, long service life, reliable coating quality and simple inspection.

The Process Step by Step

1. Alkali Cleaning

Pipes that carry oil or grease from the forming and handling process are cleaned in an alkaline solution. Oil would prevent the acid and flux from reaching the steel surface and would cause uncoated spots.

2. Pickling

The pipe is immersed in acid, normally hydrochloric acid, to dissolve mill scale and rust from the surface. Pickling must remove all scale; remaining scale creates bare patches in the coating.

3. Rinsing

Rinsing in water removes residual acid and iron salts from the surface. Incomplete rinsing can drag acid into the flux and zinc bath, causing dross and coating defects.

4. Fluxing

The pipe is dipped in a flux solution, typically zinc ammonium chloride. The flux removes the last oxide film, keeps the surface clean until dipping, and promotes wetting of the steel by the molten zinc.

5. Drying

The fluxed pipe is dried before entering the zinc bath. Moisture on the surface would flash to steam in the molten zinc and cause violent spitting, known as blasting, which creates bare spots and safety hazards.

6. Hot-Dip Galvanizing

The pipe is immersed in the zinc bath, which is typically maintained between about 445 and 465 degrees Celsius, with 450 degrees Celsius a common set point. The immersion time is controlled so that the iron-zinc reaction forms a complete alloy layer without excessive dross. In mechanized lines, pipes travel through the bath on inclined spirals and are lifted out onto the exit roller table.

7. External Wiping

As the pipe leaves the bath, compressed air or wiping rings remove excess liquid zinc from the outside surface, giving a smooth, uniform coating and controlling the final coating thickness.

8. Dragging Out

The withdrawal speed is controlled to set the coating mass: slower withdrawal leaves a heavier coating, faster withdrawal a thinner one. The speed is tuned to meet the specified coating class while keeping zinc consumption economical.

9. Internal Wiping

For pipe, the inside surface is also wiped, usually by steam or air, to remove excess zinc and give a smooth bore. The removed zinc is collected as zinc powder and recycled.

10. Water Cooling

The hot galvanized pipe is cooled, typically in a water bath held around 80 degrees Celsius, to stop the iron-zinc reaction and allow handling. Cooling conditions also affect the formation of the spangle.

11. Passivation

A passivation solution is applied to the cooled surface to delay the formation of white rust during storage and transport, especially in humid conditions.

12. Inspection and Packing

Each pipe is inspected for bare spots, drips and coating defects. Pipes with defects are reworked or rejected, and the finished pipes are bundled and packed for shipment.

Quality Control and Standards

Coating quality is verified by several checks. Coating mass and thickness are measured with a magnetic gauge per ISO 2178, and the minimum average coating mass is specified by EN ISO 1461 according to the steel thickness: about 610 g/m2 for steel over 6 mm thick, 505 g/m2 for 3 to 6 mm, 395 g/m2 for 1.5 to 3 mm, and 275 g/m2 below 1.5 mm. Adhesion is checked by bending or hammering tests that must not cause flaking. Uniformity is verified by the copper sulfate test. The pipe base itself follows the applicable pipe standard, such as GB/T 3091, EN 10217 or ASTM A53, and the certificate must state both the base standard and the coating standard.

Process step Purpose
Alkali cleaning Remove oil and grease
Pickling Remove scale and rust
Rinsing Remove acid and iron salts
Fluxing Clean surface and promote zinc wetting
Drying Prevent blasting in the zinc bath
Hot-dip galvanizing Form the zinc-iron alloy coating
Wiping and cooling Control coating thickness and stop reaction
Passivation Delay white rust during storage
Inspection Detect bare spots and coating defects

FAQ

Why is the pipe cleaned and pickled before galvanizing?

Zinc only bonds to a clean steel surface. Oil, scale and rust prevent the iron-zinc reaction and create bare, uncoated areas, so the surface must be fully cleaned and pickled before dipping.

What temperature is the zinc bath?

The zinc bath is typically maintained between about 445 and 465 degrees Celsius, with 450 degrees Celsius a common set point, to control the iron-zinc reaction and dross formation.

What is the minimum coating mass on galvanized pipe?

Per EN ISO 1461, the minimum average coating mass is 275 g/m2 for steel below 1.5 mm, rising to 610 g/m2 for steel over 6 mm thick.

Why does the pipe need fluxing before dipping?

The flux removes the thin oxide film that reforms after pickling and promotes wetting of the steel by molten zinc, ensuring a complete coating without bare spots.

How is the coating thickness measured?

Coating thickness and mass are measured with a magnetic coating gauge per ISO 2178, and adhesion is verified by bending or hammer tests per EN ISO 1461.

What causes white rust on freshly galvanized pipe?

White rust forms when the wet, reactive zinc surface is stored in humid conditions with poor ventilation. Passivation and dry storage prevent or delay it.