What are the factors that affect the corrosion resistance of SECC?

Sep 19, 2025 Leave a message

1.How does zinc layer thickness affect SECC's corrosion resistance?

How it affects the performance: The thickness of the electrolytic zinc coating directly determines the strength of the physical barrier and the sacrificial anode protection period. The thicker the zinc layer, the longer it prevents corrosive media (water, oxygen, and salt) from penetrating the steel substrate, and the longer the sacrificial protection (preferential oxidation of zinc) lasts.

Specific manifestations:
The conventional SECC zinc coating thickness is 5-20μm (8-12μm is common). If the thickness is less than 8μm, white rust (zinc oxidation product Zn(OH)₂) may appear within 1-2 months in a humid environment.

Thickening the zinc layer (e.g., 20μm or greater) can improve corrosion resistance by 30%-50%, but this increases the cost of the electrolytic process. Excessively thick zinc layers can also cause zinc peeling during subsequent stamping. Therefore, a balance must be struck between thickness and workability.

SECC

2.How does the purity and structure of the zinc layer affect the corrosion resistance of SECC?

Purity Effect: The purity of the electrolytic zinc coating (the amount of impurities such as Fe, Pb, and Cd) directly affects its electrochemical activity. Higher impurity levels increase the likelihood of "micro-batteries" forming within the zinc layer (the impurities act as cathodes and the zinc acts as anodes), accelerating localized corrosion (i.e., pitting) of the zinc.

High-purity zinc coatings (purity ≥99.9%) exhibit a weak micro-battery effect, resulting in uniform and slow corrosion and a delayed onset of white rust.

Low-purity zinc coatings (Fe content >0.5%) are susceptible to small corrosion pits forming near impurities, leading to the appearance of pitted rust within a short period of time.

Structural Effect: The electrolytic zinc coating has a columnar crystal structure. If the crystals are loosely arranged and have pores (e.g., due to unstable electrolysis current), corrosive media can penetrate directly into the substrate through these pores, bypassing the protective zinc layer and causing "interfacial corrosion" (rust between the steel substrate and the zinc layer), significantly reducing corrosion resistance.

SECC

3.What effect does passivation treatment have on the corrosion resistance of SECC?

Principle: A "passivation film" (0.1-1μm thick) is formed on the zinc surface through chemical treatment (such as chromate or chromium-free passivation). This film, consisting of a dense oxide/salt structure, not only further isolates the corrosive medium but also inhibits the electrochemical oxidation reaction of zinc (reducing the consumption rate of the sacrificial anode).

The impact of different passivation types:

Chromate passivation (traditional process): This forms a Cr³⁺/Cr⁶⁺ composite film, which offers excellent corrosion resistance. Bare zinc SECC typically shows white rust after 12-24 hours in a neutral salt spray (NSS) test, while chromate passivation can extend this to 72-120 hours. However, due to the toxicity of Cr⁶⁺, it is currently being replaced by chromium-free passivation.
Chromium-free passivation (environmentally friendly process): such as silane passivation and titanate passivation. The corrosion resistance of the formed film is slightly lower than that of chromate (white rust appears in 48-72 hours in the NSS test), but it meets environmental protection requirements and is the current mainstream.

SECC

4.What effect does anti-fingerprint treatment have on the corrosion resistance of SECC?

Principle: Applying an organic anti-fingerprint coating (0.5-2μm thick, such as acrylic resin) to the surface of the passivation film not only prevents fingerprints from remaining (improving the appearance) but also further enhances the insulation effect-essentially adding an "organic barrier" to the zinc layer and passivation film.

Performance Impact: SECC treated with anti-fingerprint treatment (such as the SECC-N2 model) can extend its neutral salt spray test duration by 30%-50% and resist mild corrosion from sweat and oil (suitable for high-contact environments such as home appliance panels and electronic chassis).

 

5.What damage may be caused during the processing and installation?

Mechanical damage (most common)
Excessive die pressure or sharp edges during stamping and bending can cause the zinc layer to peel and the passivation film to crack, exposing the steel substrate. Collision and friction during installation can also cause localized scratches. These damaged areas become "corrosion starting points." Due to the "small anode (exposed steel) - large cathode (surrounding zinc layer)" effect, the steel substrate will rapidly rust (pitting or crevice corrosion), which then spreads to the surrounding area.
Welding/Jointing Methods
The high temperatures during welding can burn away the zinc layer and passivation film near the weld. Without touch-up painting/re-plating, the weld seam will become a major corrosion hotspot.
Gaps in bolted connections (if not sealed) allow rainwater and dust to enter the gaps, causing "crevice corrosion," which corrodes 3-5 times faster than the exposed surface.