What is the production process of DC06?

Aug 25, 2025 Leave a message

As a high-grade, deep-drawing, cold-rolled steel plate, DC06's production process requires strict control of process parameters at every stage to ensure extremely low yield strength, excellent ductility, and uniform properties. The entire process, starting with steelmaking and continuing through multiple rolling, annealing, and finishing steps, focuses on achieving deep-drawability through precise composition control, rolling process optimization, and annealing microstructure control. The following is a detailed production process flow:

1. Steelmaking: Laying the Foundation for Composition
DC06 requires **ultra-low carbon (C ≤ 0.008%), low phosphorus and sulfur, and aluminum-containing grain refinement**. Therefore, the steelmaking process requires precise control of chemical composition, utilizing a combined "converter + refining" process:

1. Hot Metal Pretreatment

Removing sulfur (S ≤ 0.010%) and phosphorus (P ≤ 0.015%) from the hot metal prevents the formation of brittle inclusions during subsequent rolling.
2. Converter Smelting
Molten iron is mixed with scrap steel and oxygen top-blown to reduce the carbon content to 0.02-0.03% (initial decarburization). The manganese and other element contents are controlled (Mn ≤ 0.40%).
3. RH Vacuum Refining**

A key process! Further decarburization is performed to ≤ 0.008% in a vacuum environment (vacuum pressure ≤ 67 Pa). Aluminum (Al ≥ 0.015%) is simultaneously added for final deoxidation, grain refinement, and nitrogen fixation (to prevent nitrogen-induced age hardening).
4. Continuous Casting**
The refined steel is cast into slabs (150-250mm thick). Low superheat pouring and electromagnetic stirring are used to prevent center segregation and bubbles, ensuring uniform composition throughout the ingot.

 2. Hot Rolling: Preparation of Cold-Rolled Base Plate
DC06 cold-rolled base plate requires uniform microstructure and low hardness. The hot rolling process focuses on controlling the rolling and coiling temperatures:
1. Slab Heating
The continuous cast slab is heated in a heating furnace to 1150-1250°C to ensure homogenization of the austenite grains (to avoid performance fluctuations during subsequent rolling).
2. Rough Rolling
The slab is rolled to an intermediate bar with a thickness of 30-50mm. Multi-pass rolling with controlled reduction (15-25% reduction per pass) is used to break up coarse grains.
3. Finishing Rolling
The intermediate bar is rolled through seven continuous rolling mills to a hot-rolled strip with a thickness of 2.0-4.0mm. Controlling the final rolling temperature (850-900°C) is crucial to ensure that the steel is rolled within the austenite region. 4. **Laminar Cooling + Coiling**
After finishing rolling, the strip is rapidly cooled to 600-650°C (the ferrite transformation temperature range) using laminar cooling water, and then coiled into hot-rolled coil. This temperature range promotes uniform precipitation of ferrite grains, providing a soft substrate for subsequent cold rolling.

III. Cold Rolling: Controlling Thickness and Surface Quality
Cold rolling is the core process that determines the thickness accuracy and surface finish of DC06 steel. High reduction rolling achieves material strengthening and thickness reduction:
1. **Hot-Rolled Coil Preparation**
The hot-rolled coil surface is cleaned of iron oxide scale (using a pickling process with hydrochloric acid or sulfuric acid solution) to ensure a defect-free surface during cold rolling. 2. Cold Rolling

After pickling, the strip enters a multi-stand tandem cold mill (usually five stands) where it is rolled from 2.0-4.0mm to the target thickness (0.3-3.0mm) through continuous high-reduction rolling, achieving a total reduction of 70-90%.

- Key parameters: Rolling speed 800-1500m/min, rolling force 1000-3000kN, lubrication and cooling with rolling oil, and controlled strip surface roughness (Ra 0.4-1.6μm).
- Purpose: To refine the grain size through cold working deformation while maintaining a thickness tolerance (±0.01mm) to meet the dimensional accuracy requirements of subsequent deep drawing.

 IV. Annealing: Restoring Plasticity and Optimizing Deep Drawing Performance
After cold rolling, the strip increases in hardness and decreases in plasticity due to cold work hardening. Annealing is necessary to relieve stress and soften the microstructure. This is key to achieving high elongation for DC06:
1. Continuous Annealing (CAPL or CGL Production Line)**
DC06 typically utilizes continuous annealing (an alternative to traditional bell annealing, which is more efficient and provides more uniform performance). The process curve is divided into four stages:
- Preheating Stage**: The strip is heated from room temperature to 400-500°C, slowly increasing the temperature to avoid thermal stress.
-  Stage: Rapidly heating to 750-800°C (above the recrystallization temperature) to fully recrystallize the grains deformed by cold rolling.
- Soaking Stage: The strip is held at 750-800°C for 30-60 seconds to promote uniform growth of recrystallized grains (average grain size 15-25μm).
- Cooling Stage: Rapid cooling to 600-650°C followed by slow cooling to below 200°C controls the stability of the ferrite structure and prevents carbide precipitation that could reduce plasticity.

2. Tempering Rolling**
After annealing, the strip undergoes a light rolling (reduction ratio of 0.5-3%) to:
- Eliminate the post-annealing yield plateau (to prevent "Lüders lines" and surface defects during deep drawing);
- Adjust the strip's straightness (to control wavy shapes) and surface roughness (through work roll texture transfer, optimizing subsequent coating adhesion).

 V. Finishing: Ensuring Final Quality

1. **Splitting/Trimming**
Splitting large strip into smaller coils (weighing 5-30 tons) as required by the customer, while simultaneously trimming burrs and defects from the strip edges to ensure width accuracy.

2. Inspection and Packaging**
Surface defects (scratches, pitting, etc.) are inspected through online flaw detection (such as eddy current testing). Acceptable results are then coated with anti-rust oil and paper, and finally secured with coil packaging tape to prevent damage during transportation.

Summary of Core Process Features
The core of DC06 production is full-process control centered around "deep-drawing performance":
- Composition End**: Ultra-low carbon and aluminum refinement lay the foundation for plasticity;
- Hot-rolling End**: Controlled coiling temperature creates a uniform ferrite base;
- Cold-rolling End**: High reduction ensures precision and provides a driving force for recrystallization;
- Annealing End**: Complete recrystallization and elimination of the yield plateau achieve low yield and high elongation.

The synergistic effect of this series of processes ultimately gives DC06 excellent deep-drawing properties: easy stretching, no deformation, and no cracking, meeting the forming requirements of complex parts.