1.What is "white rust"?
White rust is a corrosion product of zinc on the surface of galvanized coatings, and its main components are basic zinc carbonate or zinc hydroxide. It is usually formed when galvanized coils are exposed to humid, poorly ventilated environments (such as being rained on or soaked in condensation), causing zinc to react with oxygen and moisture.

2.What are the specific effects of white rust on welding quality?
Porosity
This is the most significant and common problem. White rust (a mixture of moisture and corrosion products) rapidly decomposes upon contact with the high temperatures of the welding arc, producing large amounts of water vapor (H₂O) and carbon dioxide (CO₂).
These gases cannot escape before the molten pool solidifies and become trapped in the weld metal, forming numerous pores.
Harm: Porosity severely reduces the effective cross-sectional area of the weld, leading to a significant decrease in the weld's mechanical properties (such as strength, toughness, and fatigue strength), becoming a potential fracture initiation point.
Increased Weld Spatter
The presence of white rust disrupts the stability of the arc and causes the molten metal to become irregular during the transition.
This results in severe spatter, wasting welding materials, contaminating the workpiece surface, and increasing the workload of post-weld cleaning.
Insufficient Fusion and Penetration
The white rust layer acts as a "barrier" on the surface of the base metal to be welded. The arc energy is first consumed on this contaminant layer, rather than being directly used to melt the base metal.
This can lead to insufficient penetration, meaning the weld seam fails to fully penetrate to the required depth, or even result in incomplete fusion defects, making the weld joint weak.

3.How to mechanically clean galvanized coils with white rust?
Tools: Use an angle grinder with a wire brush, grinding wheel, or louvered blades.
Scope: The cleaning area should be wider than the weld area; generally, a bright metal surface must be exposed within 20-30 mm on each side of the weld.
Note: After cleaning, it is best to blow away the dust with compressed air.

4.How is chemical cleaning performed?
Specialized zinc plating cleaners or diluted acidic solutions (such as hydrochloric acid) can be used to dissolve white rust and the zinc layer.
Disadvantages: The process is cumbersome, involves chemical hazards, and requires thorough rinsing and drying of the chemicals before welding; otherwise, residues can introduce new problems. It is rarely used for pre-welding treatment in industrial production.
5.How should the welding process be adjusted?
Increase current/heat input appropriately: Because zinc's boiling point (907°C) is much lower than steel's melting point (approximately 1500°C), the zinc layer will vaporize first under the action of the arc, consuming some energy. Appropriately increasing the heat can ensure sufficient penetration into the base material.
Slightly reduce welding speed: Giving the gas more time to escape from the molten pool helps reduce porosity.
Use appropriate welding techniques: For example, in shielded metal arc welding (SMAW), a short arc and straight electrode movement can be used; in gas shielded welding (GSAW), a slightly higher gas flow rate and a push-pull technique can be used.