What are the common surface defects of galvanized steel strip?

Jun 23, 2025 Leave a message

1.What are the types and causes of substrate defects before plating?

Rolling scale residue: incomplete pickling
Edge burrs: slitting machine tool clearance > 10% of plate thickness
Roller indentation: roller surface damage or foreign matter pressed into the roller

Galvanized steel strip

2.What are the core defect types in the galvanizing process?

Defects in uniformity of coating: zinc fluctuations, uneven zinc flowers, and missed plating.
Defects in bonding strength of coating: zinc slag
Surface contamination defects: oil spots

 

3.What are the types of post-processing defects and their causes?

Passivation spot: passivation solution pH>4.5 resulting in uneven film formation
White rust: storage humidity>70% + Cl⁻ erosion
Blackening: chromate passivation film is too thick

Galvanized steel strip

4.What are the types and causes of transportation and storage defects?

Coil core collapse: inner diameter of steel coil < 508mm, insufficient load bearing
Edge scratches: steel coil collision during transportation
Seawater corrosion: salt spray intrusion into shipping containers

Galvanized steel strip

5.What are the defect detection and grading criteria?

Online detection technology: Laser confocal microscope: Identify zinc slag (resolution 1μm)
Infrared thermal imager: Monitor coating uniformity (temperature difference > 3℃ alarm)
Offline standard: European standard EN 10346: Allow ≤ 3 defects/m² (automobile outer panel)
American standard ASTM A924: Zinc fluctuation height < 0.5% plate thickness